PET composite material and preparation method thereof
Through the preparation method of PET composite materials, PET copolyester and inorganic fillers are used to reduce the cold crystallization temperature of PET, solve the problem of recycling and processing of waste PET pressure-sensitive tape, and achieve efficient use of resources and environmental protection.
Patent Information
- Application Number
- CN202410571932.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-10
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-05-10
AI Technical Summary
It is difficult to effectively recycle waste PET pressure-sensitive tape with existing technology, and the cold crystallization temperature of PET material is high, resulting in processing difficulties and resource waste.
Using the preparation method of PET composite materials, by melting waste pressure-sensitive adhesive products and adding alcoholysis agent and catalyst to form PET copolyester, combining inorganic fillers and PET, lowering the cold crystallization temperature point of PET, eliminating its weaknesses, and realizing Overall recycling of pressure-sensitive adhesive layers.
It achieves efficient recycling of waste PET and pressure-sensitive adhesive products, reduces the cold crystallization temperature of PET composite materials, increases the mold temperature, enhances the mechanical properties of the material, simplifies the process, and reduces environmental pollution.
Smart Images

Figure BDA0004831109070000131
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of recycling waste PET materials, and in particular, relates to a PET composite material and a preparation method thereof. Background Art
[0002] PET polyester film is an important new material in the current industrial intermediate material and future strategic emerging industries. It is a polymer film material with excellent comprehensive performance. It is widely used as a pressure-sensitive adhesive substrate to prepare pressure-sensitive tapes. With the widespread application of pressure-sensitive tapes in packaging and other fields, the waste of pressure-sensitive tapes is increasing year by year, and the pollution and waste of resources caused to the environment are becoming increasingly prominent, becoming a problem that cannot be ignored at present and in the future. The recycling of traditional PET pressure-sensitive tapes requires the removal of the adhesive layer adhering to PET before recycling, and the degumming process is often complicated and cumbersome. The treatment of these discarded PET tapes is more troublesome, and many places even adopt incineration. On the one hand, the incineration treatment method will cause air pollution, and on the other hand, it does not achieve the recycling of materials and wastes energy.
[0003] Patent application CN103374791A discloses a process for manufacturing non-woven fabrics from waste PET: the recycled PET film is crushed and dried; the crushed PET is stirred, and ethylene-octanoic acid copolymer is added to form a mixture; the mixture is fed into a twin-screw extruder to extrude and plasticize into particles, and subsequent processing, which only involves the recycling of PET film and cannot be applied to the recycling of PET tapes containing pressure-sensitive adhesive layers.
[0004] Patent application CN106009545A discloses a method for producing film sheets by directly melting the recycled waste PET, which includes the following steps: 1) crushing and decolorizing the waste PET, heating and melting, adding PET, PBT, antioxidants, flame retardants, and chain extenders, raising the temperature to 290°C, and treating for 160-170s under the combined action of microwaves and ultrasound; 2) directly performing film pressing, first hot pressing and then cold pressing during the pressing process to obtain a finished film. This method requires crushing and decolorizing the PET, which is a complex process and does not involve the treatment of the pressure-sensitive adhesive in the PET tape.
[0005] Patent application US20220152904A1 discloses a method for producing biaxially oriented polyester (BOPET) stripping using recycled PET, which includes the following steps: pre-cleaning the recycled PET, performing primary washing of the recycled PET with a solvent to remove contaminants, brushing the PET to remove dust and unnecessary materials, removing impurities in the particles through a filtration process, and decolorizing the particles through a clay bed, and then glycolyzing the pre-cleaned PET to obtain monomers, and then condensing the monomers in an autoclave. This method requires pre-cleaning of the recycled PET, and the process is complicated. For PET pressure-sensitive tape, the cleaned adhesive layer is difficult to handle, and it is easy to pollute the environment.
[0006] Patent application KR102611876B1 discloses the use of waste PET fragments to prepare PET film, which requires separating the waste PET and washing the inorganic particles, color sorting, drying, crushing, washing with a non-solvent solution, drying and separating from the metal particles, and then adding a molding improver (TEP) to the mixing equipment, adding SiO2, melt mixing, and then processing into recycled PET film. This method requires the treatment of waste PET, the steps are complicated, and it does not involve the recycling of pressure-sensitive adhesives in PET tapes.
[0007] In addition, PET itself has a cold crystallization temperature point (Tcc), which is usually in the range of 136℃~147℃, which cannot meet the mold temperature requirements of normal injection molding molds. During the injection molding process, the mold temperature controller is forced to be installed to heat the molding mold and keep the temperature constant to the cold crystallization temperature range of PET. Although the influence of the cold crystallization temperature point of PET can be temporarily eliminated, once the ambient temperature of the PET product reaches the cold crystallization temperature, secondary crystallization will occur due to the memory effect of the cold crystallization temperature point of PET. At this time, stress cracking or direct melting will occur, which is the most fatal weakness of PET.
[0008] Therefore, if these waste PET substrates can be recycled and their cold crystallization temperature can be lowered, it will be of great significance to energy conservation, environmental protection and improving product performance. Summary of the invention
[0009] Based on this, the present invention aims to overcome at least one defect of the prior art and provide a PET composite material, which is not only prepared from waste PET materials, but also has excellent performance and can meet the performance requirements of PET products.
[0010] Another object of the present invention is to provide a method for preparing a PET composite material, which can fully recycle waste PET film and PET pressure-sensitive tape, thereby realizing the recycling of two major waste PET materials.
[0011] The technical scheme is as follows: a PET composite material, which contains, by weight, 50 to 100 parts of PET, 5 to 20 parts of inorganic fillers and 5 to 30 parts of PET copolyester; wherein the PET copolyester is obtained by melting a waste pressure-sensitive adhesive product, adding an alcoholysis agent and a catalyst, and then vacuum polycondensing, wherein the waste pressure-sensitive adhesive product comprises a PET matrix and a pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer comprises a copolyester elastomer, the copolyester elastomer is a copolymer of a carboxyl-terminated polyester and a non-crystalline carbon dioxide-based polyester diol, and the number average molecular weight of the PET copolyester is 20,000 to 50,000.
[0012] The present invention also relates to a method for preparing the above PET composite material, comprising the following steps:
[0013] (1) melting the waste pressure-sensitive adhesive product, adding an alcoholysis agent and a catalyst, and then polycondensing to obtain the PET copolyester;
[0014] (2) Processing the components other than the PET copolyester into a premelt; adding the PET copolyester obtained in step (1) into the premelt, followed by melting, heat preservation, and extrusion to obtain the PET composite material.
[0015] The pressure-sensitive adhesive product of the present invention has a PET matrix, and the pressure-sensitive adhesive layer comprises a copolyester elastomer, which is a copolymer of a carboxyl-terminated polyester and a non-crystalline carbon dioxide-based polyester diol, and is a material with good degradation performance. The pressure-sensitive adhesive tape is completely melted by high temperature, that is, the base film and the pressure-sensitive adhesive layer are completely melted, and after adding a catalyst and an alcoholysis agent, the pressure-sensitive adhesive tape is alcoholysed into small molecular monomers, and a new PET copolyester is formed by polycondensation. The pressure-sensitive adhesive product containing the above-mentioned type of copolyester elastomer does not need to peel off the pressure-sensitive adhesive layer, and it will not be necessary to alcoholyze PET into monomers or oligomers and then react with new components, which greatly simplifies the chemical conversion step. Compared with PET materials, the PET copolyester formed by polycondensation has lower cold crystallization temperature points, hot crystallization temperature points, and glass transition temperatures. The reason is that amorphous segments are introduced into this PET copolyester, which makes the glass transition temperature of PET lower, softer, and reduces the cold crystallization temperature of PET. Melting and compounding this PET copolyester with PET can lower the cooling crystallization temperature of PET, eliminate the weaknesses of PET, and reduce the spatial steric hindrance of PET. The molding mold temperature of the obtained PET composite material is higher than the cold crystallization temperature, and PET will not undergo secondary crystallization, which is conducive to the processing of PET materials.
[0016] Therefore, the beneficial effects of the present invention are as follows: the technical scheme described in the present invention can realize the recycling of waste PET and waste pressure-sensitive adhesive products, wherein the recycling of waste pressure-sensitive adhesive products does not require the degumming treatment of the pressure-sensitive adhesive layer first, and the overall recycling of the pressure-sensitive adhesive products can be directly realized, and the recycled PET composite material has a low crystallization temperature, which can eliminate the weaknesses of PET. After the PET composite material reduces the cold crystallization temperature, the molding mold temperature is higher than the cold crystallization temperature, and PET will not undergo secondary crystallization, which is conducive to the processing of PET materials, and the prepared PET composite material has excellent mechanical properties. DETAILED DESCRIPTION
[0017] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific implementation methods.
[0018] For the PET composite material of the present invention, in one embodiment, the 50-100 parts of PET include waste PET, and the waste PET mainly comes from beverage bottles, films, laminates, tapes, high-grade sheets, fibers, etc., and medical supplies, such as PET in syringes and containers. In addition, the PET may not contain waste PET. The molecular weight of the PET is less than 50,000, and may be 45,000, 40,000, 35,000, 30,000, 25,000, 20,000, etc.
[0019] In one embodiment, the copolyester elastomer comprises a hard segment carboxyl-terminated polyester and a degradable soft segment non-crystalline carbon dioxide-based polyester diol. The soft segment non-crystalline carbon dioxide-based polyester diol is a CO2-based diol, derived from a third type of carbon source, with a fast degradation rate and a high degradation rate. Since the soft segment carbon dioxide-based polyester diol used is a non-crystalline diol, it has poor cohesion and cannot be used in the field of pressure-sensitive adhesives. Therefore, a degradable hard segment carboxyl-terminated polyester with a specific molecular weight is introduced to increase its cohesive strength. Since the hard segment is also degradable, the hard segment part can also be degraded, so that the copolyester elastomer obtained by polymerizing the hard segment carboxyl-terminated polyester and the soft segment non-crystalline carbon dioxide-based polyester diol is completely degradable. The polyester is polymerized from a C3-C7 dibasic acid and a C3-C7 diol, and accounts for 10 to 30% by mass of the copolyester elastomer. The number average molecular weight of the polyester is 1100 to 3000. The non-crystalline carbon dioxide-based polyester diol is a copolymer of polypropylene carbonate diol, and the number average molecular weight of the copolyester elastomer is 30,000 to 50,000.
[0020] Since the hard segment contains carboxyl groups, it can be used as a physical crosslinking point to form a copolyester elastomer with the soft segment carbon dioxide-based polyester diol, thereby improving the cohesive strength of the overall resin, so that it can be used in the field of pressure-sensitive adhesives to meet the bonding properties of pressure-sensitive adhesives. In order to obtain the required performance, the mass ratio of the hard segment to the elastomer should be more than 10%. As its content increases, the cohesive properties of the copolyester elastomer will increase, but too high a hard segment content will lead to an increase in the degree of phase separation, and then the performance of the elastomer will decrease, causing the subsequent pressure-sensitive adhesive performance to decrease. At the same time, if the hard segment content is too high, the physical entanglement of the elastomer will also increase, and then the degradation rate of the elastomer will decrease, so the mass ratio of the hard segment is controlled below 30%. Specifically, the proportion of the hard segment can be 12%, 14%, 16%, 18%, 20%, 22%, 24%, 26% or 28%.
[0021] In addition, the molecular weight of the hard segment, soft segment, and copolyester elastomer will also affect the performance of the degradable copolyester elastomer. For the hard segment, the higher the molecular weight, the stronger the crystallinity, and the stronger the ability to serve as a physical crosslinking point. In order to meet the performance requirements, the number average molecular weight of the hard segment is above 1100, but the crystallinity caused by the excessively high molecular weight is too strong, which makes the microphase separation degree of the degradable copolyester elastomer too large, which in turn leads to a decrease in the performance of the degradable copolyester elastomer and a decrease in the performance of the subsequent pressure-sensitive adhesive. The number average molecular weight of the hard segment should be controlled below 3000. Specifically, the number average molecular weight of the hard segment can be 1200, 1400, 1600, 1800, 2000, 2200, 2400, 2600, 2800 or 2900. For the soft segment, when the molecular weight is too small, the chain segment is too short, and the degradable copolyester elastomer loses elasticity. Therefore, its number average molecular weight is at least 2000. When the molecular weight is too large, it is equivalent to a decrease in the hard segment content, and the strength of the degradable copolyester elastomer decreases, affecting the subsequent use as a pressure-sensitive adhesive matrix resin. The number average control amount should be controlled below 3000. Specifically, the number average molecular weight of the soft segment can be 2100, 2200, 2300, 2400, 2500, 2600, 2700, 2800 or 2900. For the copolyester elastomer, its molecular weight needs to be above 30000 so as to have the required cohesion, but when the molecular weight is too large, it will lead to poor degradation performance, so it needs to be controlled below 50000. The number average molecular weight of the copolyester elastomer can be 32000, 34000, 36000, 38000, 40000, 42000, 44000, 46000 or 48000.
[0022] By controlling the molecular weight of the soft and hard segments of the degradable copolyester elastomer, the segment content and the overall molecular weight of the copolyester, the copolyester elastomer can have excellent cohesive strength and degradability, and the degradable polyester pressure-sensitive adhesive has both excellent bonding and degradation properties. By mixing the degradable copolyester elastomer with a tackifying resin, a plasticizer, etc., the prepared degradable polyester pressure-sensitive adhesive has excellent initial adhesion, lasting adhesion, high peel strength, and high degradation rate, and it is not easy to have residual adhesive after the pressure-sensitive adhesive is peeled off.
[0023] In one embodiment, the carboxyl-terminated polyester is polymerized from a C3-C7 dibasic acid and a C3-C7 diol.
[0024] In one embodiment, the carboxyl-terminated polyester is polybutylene succinate (PBS), and the non-crystalline carbon dioxide-based polyester diol is polypropylene carbonate diol (PPC). PBS and PPC are novel polymer degradable materials, and the degradation mechanism of PBS is: first, by the hydrolysis of CO bonds, and then further degraded under the action of enzymes. PBS is a crystalline material, which can be used as a physical crosslinking point to form a copolyester elastomer with polycarbonate, thereby improving the cohesive strength of the overall resin, so that it can be applied in the field of pressure-sensitive adhesives to meet the bonding properties of pressure-sensitive adhesives, and the PBS synthetic raw material comes from biomass, which is a second-class carbon source, and the degradation performance is also good. The PPC segment is a CO2-based diol, which comes from a third-class carbon source, has a fast degradation rate, and a high degradation rate.
[0025] In one embodiment, the PET is preferably 70 to 90 parts, the inorganic filler is preferably 10 to 20 parts, and the PET copolyester is preferably 10 to 30 parts.
[0026] In one embodiment, the cooling crystallization temperature of the PET composite material is 90-135°C, preferably 105-130°C, and more preferably 110-120°C. The number average molecular weight of the PET copolyester is 15,000-50,000, preferably 20,000-45,000, and more preferably 30,000-40,000.
[0027] In one embodiment, the PET composite material further contains 0.2 to 1 parts of a dispersant, 0.2 to 1 parts of an antioxidant, and may also contain 0.1 to 10 parts of any additives in the art, such as a flame retardant, a toughening agent, a coupling agent, a lubricant, and the like.
[0028] In one embodiment, the alcoholysis agent is one or more of methanol, ethanol, ethylene glycol, propylene glycol, butylene glycol and pentanediol, for example, butylene glycol, and the mass ratio of the alcoholysis agent alcohol to the pressure-sensitive adhesive product is (1-2) : 1, preferably (1.3-1.8): 1.
[0029] In one embodiment, the catalyst is tetrabutyl titanate, tetraisopropyl titanate or p-toluenesulfonic acid, and the amount of the catalyst used is 0.01-1% of the mass of the pressure-sensitive adhesive product, preferably 0.3‰-1‰.
[0030] In one embodiment, the pressure-sensitive adhesive product is a degradable adhesive tape, adhesive stick or adhesive roll.
[0031] In one embodiment, the inorganic filler is one or more of talc, titanium dioxide, heavy calcium titanate, wollastonite, mica, kaolin, potassium titanate whiskers, calcium carbonate whiskers, barium sulfate and silicon dioxide, and the content of the inorganic filler is 5 to 30 parts, preferably 8 to 20 parts, and more preferably 10 to 18 parts.
[0032] In one embodiment, the dispersant is a TA-based lubricating dispersant or an ethylene-acrylate copolymer.
[0033] In one embodiment, the antioxidant is antioxidant 1010, antioxidant 168 or antioxidant 1076.
[0034] In one embodiment, the pressure-sensitive adhesive layer is a degradable pressure-sensitive adhesive layer, which comprises, by weight: 20 to 80 parts of a copolyester elastomer, preferably 30 to 70 parts, more preferably 50 to 60 parts; 20 to 50 parts of a tackifying resin; 1 to 10 parts of
[0035] a plasticizer; and optionally additives.
[0036] In one embodiment, the tackifying resin is one or more of natural rosin, hydrogenated rosin, disproportionated rosin, esterified rosin, C5 petroleum resin, C9 petroleum resin, and terpene resin, and the content of the tackifying resin is preferably 30 to 50 parts, more preferably 40 to 50 parts;
[0037] In one embodiment, the plasticizer is one or more of epoxidized soybean oil, linseed oil, castor oil, and palm oil.
[0038] In one embodiment, the additive includes an antioxidant, and the antioxidant is one or more of tris(2,4-di-tert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, di(tridecanol)thiodipropionate, and pentaerythritol tetrakis{3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate}.
[0039] In one embodiment, the PET includes waste PET, but is not limited to waste PET. There is no specific requirement for the molecular weight of the PET, and it can be a conventional molecular weight in PET composite materials. The molecular weight can also be 10,000 to 100,000, or 15,000 to 80,000, or 20,000 to 70,000, or 25,000 to 60,000, or 30,000 to 50,000, or 35,000 to 45,000.
[0040] In one embodiment, the tensile strength of the PET composite material is 120-160 MPa.
[0041] In one embodiment, the elongation at break of the PET composite material is 3-12%.
[0042] In one embodiment of the method for preparing a PET composite material of the present invention, in step 1), the waste pressure-sensitive adhesive product is melted at 260-280° C., stirred for 3-4 hours, an alcoholysis agent and a catalyst are added, and vacuum polycondensation is performed for 1-6.5 hours to obtain the PET copolyester.
[0043] In one embodiment, in step (2), the PET copolyester obtained in step (1) is introduced from the die head and melt-blended and extruded with the pre-melt. The melt-blending conditions are: temperature 200-240° C., and extruder speed of 100-500 rpm.
[0044] In one embodiment, the specific steps of melt-blending and extruding the molten copolyester and the premelt in a twin-screw extruder in step (2) are as follows: 10 to 30 parts of the PET copolyester obtained in step (1) are introduced from the die head and melt-blended and extruded with 70 to 90 parts of the premelt in a twin-screw extruder, and the melt-blending conditions are: temperature 210 to 230° C., and twin-screw extruder speed 200 to 400 rpm.
[0045] In one embodiment, the premixing conditions in step (2) are: temperature 25±5°C, twin-screw extrusion, rotation speed 50-1500 rpm, and premixing time 3-10 minutes. More preferably, the rotation speed is 80-200 rpm.
[0046] In one embodiment, in the step (2), after extrusion, the material is pulled and cooled and then cut into pellets or sheets.
[0047] Example
[0048] The embodiments of the present invention are only used for illustrative description and should not be construed as limiting the present invention.
[0049] For simplicity, only some numerical ranges are explicitly disclosed herein. However, any lower limit can be combined with any upper limit to form an unambiguous range; and any lower limit can be combined with other lower limits to form an unambiguous range, and any upper limit can be combined with any other upper limit to form an unambiguous range. In addition, although not explicitly stated, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unambiguous range.
[0050] The above application content of the present invention is not intended to describe each disclosed embodiment or each implementation in the present invention. The following description more specifically illustrates exemplary embodiments. In many places throughout the application, guidance is provided by a series of examples, which can be used in various combinations. In each example, enumeration is only used as a representative group and should not be interpreted as exhaustive.
[0051] Unless otherwise specified, the raw materials used in the following examples are common commercially available products.
[0052] The waste pressure-sensitive adhesive products described in the following examples are waste pressure-sensitive adhesive tapes produced by our company. The specific components of the pressure-sensitive adhesive tape are a PET matrix and a pressure-sensitive adhesive layer.
[0053] The preparation process of the pressure-sensitive adhesive tape 1 used in the following Examples 1 to 5, 8 to 9 is as follows:
[0054] (1) Preparation of carboxyl-terminated polybutylene succinate
[0055] 40 parts of 1,4-butanediol and 60 parts of succinic acid were put into a reactor, then heated to 165°C, and 0.3wt% of the total mass of 1,4-butanediol and succinic acid was added to the catalyst tetrabutyl titanate, and then reacted for about 3 hours, and then heated to 180°C for about 1 hour, and then heated to 205°C for vacuum polycondensation for 2 hours, and the acid ester was tested. The acid value was tested to be 70.125mgKOH / g (the calculated number average molecular weight was 1600, and the calculation formula was: wherein y is an acid value), and after cooling to room temperature, carboxyl-terminated polybutylene succinate is obtained.
[0056] (2) Preparation of copolyester elastomer
[0057] 18 parts of carboxyl-terminated polybutylene succinate and 82 parts of non-crystalline carbon dioxide-based polyester diol (polypropylene carbonate diol, molecular weight of about 2500, hydroxyl value of about 44.88 mgKOH / g) were put into a reactor, then heated to 180°C, 0.2wt% of the total mass of carboxyl-terminated polybutylene succinate and non-crystalline carbon dioxide-based polyester diol catalyst tetrabutyl titanate was added, and the reaction was continued for 2 hours, and then the temperature was raised to 220°C for 3 hours, and then vacuum polycondensed for 4 hours, and cooled to room temperature to obtain a degradable copolyester elastomer. The molecular weight of the degradable copolyester elastomer was tested, and the number average molecular weight of the degradable copolyester elastomer was measured to be about 35,000.
[0058] (3) Preparation of pressure-sensitive adhesive solution
[0059] 50 parts of a degradable copolyester elastomer, 45 parts of a tackifying resin rosin, 5 parts of a plasticizer epoxy soybean oil, and 0.15 parts of an antioxidant tris(2,4-di-tert-butylphenyl)phosphite were mixed, stirred at 130° C. for 3 hours, then cooled to room temperature, and then a chloroform solution was added to obtain a degradable pressure-sensitive adhesive solution with a solid content of 20 wt%;
[0060] (4) Preparation of pressure-sensitive adhesive tape
[0061] The degradable pressure-sensitive adhesive solution was coated on the PET base film by a coating machine and kept at 80° C. for 10 min to obtain a degradable pressure-sensitive adhesive tape 1 with a pressure-sensitive adhesive layer thickness of about 15 μm.
[0062] The preparation process of the pressure-sensitive adhesive tape 2 used in the following Example 6 is as follows:
[0063] (1) Preparation of carboxyl-terminated polybutylene succinate
[0064] 45 parts of 1,4-butanediol and 65 parts of succinic acid were put into a reactor, then heated to 165°C, and 0.5wt% of the total mass of 1,4-butanediol and succinic acid was added as catalyst tetrabutyl titanate, and then reacted for about 4 hours, and then heated to 180°C for about 2 hours, and then heated to 220°C for vacuum polycondensation for 4 hours, and its acid ester was tested. The acid value was tested to be 38.7mgKOH / g (the calculated number average molecular weight was 2900), and carboxyl-terminated polybutylene succinate was obtained after cooling to room temperature.
[0065] (2) Preparation of copolyester elastomer
[0066] 18 parts of hard segment polyester and 82 parts of soft segment non-crystalline carbon dioxide-based polyester diol (polypropylene carbonate diol, molecular weight of about 2500, hydroxyl value of about 44.88 mgKOH / g) were put into a reactor, then heated to 180°C, carboxyl-terminated polybutylene succinate and non-crystalline carbon dioxide-based polyester diol were added, and the catalyst tetrabutyl titanate was added, which was reacted for 2 hours, and then heated to 220°C for 4 hours, and then vacuum polycondensed for 6 hours, and cooled to room temperature to obtain a degradable copolyester elastomer. The molecular weight of the degradable copolyester elastomer was tested, and the number average molecular weight of the degradable copolyester elastomer was measured to be about 49,000.
[0067] (3) Preparation of pressure-sensitive adhesive solution: the same as step (3) of the preparation process of pressure-sensitive adhesive tape 1.
[0068] (4) Preparation of pressure-sensitive adhesive tape: The same as step (4) of the preparation process of pressure-sensitive adhesive tape 1.
[0069] The preparation process of the pressure-sensitive adhesive tape 3 used in the following Example 7 is as follows:
[0070] (1) Preparation of carboxyl-terminated polybutylene succinate: The same as step (1) of the preparation process of pressure-sensitive adhesive tape 1.
[0071] (2) 10 parts of carboxyl-terminated polybutylene succinate and 90 parts of soft segment non-crystalline carbon dioxide-based polyester diol (polypropylene carbonate diol, molecular weight of about 2500, hydroxyl value of about 44.88 mgKOH / g) are put into a reaction kettle, then the temperature is raised to 190°C, 0.1wt% of the total mass of carboxyl-terminated polybutylene succinate and non-crystalline carbon dioxide-based polyester diol catalyst tetrabutyl titanate is added, and the reaction is carried out for 2 hours, and then the temperature is raised to 210°C for reaction for 3 hours, and then vacuum polycondensation is carried out for 3 hours, and the degradable copolyester elastomer is obtained after cooling to room temperature. The molecular weight of the degradable copolyester elastomer is tested, and the number average molecular weight of the degradable copolyester elastomer is measured to be about 32,000.
[0072] (3) Preparation of pressure-sensitive adhesive solution: the same as step (3) of the preparation process of pressure-sensitive adhesive tape 1.
[0073] (4) Preparation of pressure-sensitive adhesive tape: The same as step (4) of the preparation process of pressure-sensitive adhesive tape 1.
[0074] Example 1
[0075] A method for preparing a PET composite material using waste PET and a pressure-sensitive adhesive tape comprises the following steps:
[0076] (1) The waste pressure-sensitive adhesive tape 1 was melted at 260° C., stirred for 3 h, and then an alcoholysis agent and a catalyst, tetrabutyl titanate, were added, and then vacuum polycondensed for 5 h to obtain PET copolyester, wherein the amount of the alcoholysis agent was 150% of the mass of the pressure-sensitive adhesive tape and the amount of the catalyst was 0.5‰ of the mass of the waste pressure-sensitive adhesive tape; the molecular weight of the prepared PET copolyester was determined to be about 28,000.
[0077] (2) 80 parts of waste PET (PET film with a number average molecular weight of about 40,000), 15 parts of talcum powder, 0.5 parts of dispersant TA100, and 0.5 parts of antioxidant 1010 are premixed to obtain a premelt, and the premixing conditions are: temperature 25°C, twin-screw extrusion, rotation speed of about 100 rpm, and premixing time 5 minutes; 20 parts of the PET copolyester obtained in step (1) are melted at 280°C and kept warm for 15 minutes, and the molten PET copolyester is introduced from the die head and melt-blended and extruded with the premelt in a twin-screw extruder, and the melt-blending conditions are: temperature 220°C and twin-screw extruder rotation speed 300 rpm; and the pellets are cut into pellets after traction and cooling to obtain a copolyester reinforced PET composite material.
[0078] Example 2
[0079] A method for preparing a PET composite material using waste PET and a pressure-sensitive adhesive tape comprises the following steps:
[0080] (1) A discarded pressure-sensitive adhesive tape was melted at 270°C, stirred for 3.5 hours, and an alcoholysis agent and a catalyst, tetrabutyl titanate, were added, and vacuum polycondensed for 6.5 hours to obtain PET copolyester, wherein the amount of the alcoholysis agent was 160% of the mass of the pressure-sensitive adhesive tape and the amount of the catalyst was 0.3‰ of the mass of the discarded pressure-sensitive adhesive tape; the molecular weight of the prepared PET copolyester was determined to be about 30,000.
[0081] (2) 80 parts of waste PET (PET film with a number average molecular weight of about 40,000), 15 parts of talcum powder, 0.5 parts of dispersant TA100, and 0.5 parts of antioxidant 1010 are premixed to obtain a premelt, and the premixing conditions are: temperature 25°C, twin-screw extrusion, rotation speed of about 100 rpm, and premixing time 3 to 10 minutes; 20 parts of the PET copolyester obtained in step (1) are melted at 260°C and kept warm for 10 minutes, and the molten PET copolyester is introduced from the die head and melt-blended and extruded with the premelt in a twin-screw extruder, and the melt-blending conditions are: temperature 270°C and twin-screw extruder rotation speed 300 rpm; and the pellets are cut into pellets after traction and cooling to obtain a copolyester reinforced PET composite material.
[0082] Example 3
[0083] A method for preparing a PET composite material using waste PET and a pressure-sensitive adhesive tape comprises the following steps:
[0084] (1) A discarded pressure-sensitive adhesive tape No. 1 was melted at 275°C, stirred for h, and then an alcoholysis agent and a catalyst, tetrabutyl titanate, were added, and then vacuum polycondensed for 3.5 h to obtain PET copolyester, wherein the amount of alcoholysis agent used was 180% of the mass of the pressure-sensitive adhesive tape. The amount of catalyst used was 1‰ of the mass of the discarded pressure-sensitive adhesive tape; the molecular weight of the prepared PET copolyester was determined to be about 26,000.
[0085] (2) 80 parts of waste PET (PET film with a number average molecular weight of about 40,000), 15 parts of talcum powder, 0.5 parts of dispersant TA100, and 0.5 parts of antioxidant 1010 are premixed to obtain a premelt, and the premixing conditions are: temperature 25°C, twin-screw extrusion, rotation speed of about 100 rpm, and premixing time 7 minutes; 20 parts of the PET copolyester obtained in step (1) are melted at 270°C and kept warm for 20 minutes, and the molten PET copolyester is introduced from the die head and melt-blended and extruded with the premelt in a twin-screw extruder, and the melt-blending conditions are: temperature 220°C and twin-screw extruder rotation speed 300 rpm; and the pellets are cut into pellets after traction and cooling to obtain a copolyester reinforced PET composite material.
[0086] Example 4
[0087] A method for preparing a PET composite material using waste PET and a pressure-sensitive adhesive tape comprises the following steps:
[0088] (1) The discarded pressure-sensitive adhesive tape 1 was melted at 280°C, stirred for 4 hours, and then an alcoholysis agent and a catalyst, tetrabutyl titanate, were added, and then vacuum polycondensed for 5 hours to obtain PET copolyester, wherein the amount of the alcoholysis agent was 150% of the mass of the pressure-sensitive adhesive tape. The amount of the catalyst was 0.5‰ of the mass of the discarded pressure-sensitive adhesive tape. The molecular weight of the prepared PET copolyester was determined to be about 28,000.
[0089] (2) 90 parts of waste PET (PET film with a number average molecular weight of about 40,000), 20 parts of talcum powder, 1 part of dispersant TA100, and 1 part of antioxidant 1010 are pre-mixed to obtain a pre-melt, and the pre-mixing conditions are: temperature 25°C, twin-screw extrusion, rotation speed of about 100 rpm, and pre-mixing time 3 to 10 minutes; 10 parts of the PET copolyester obtained in step (1) are melted at 280°C and kept warm for 5 minutes, and the molten PET copolyester is introduced from the die head and melt-blended and extruded with the pre-melt in a twin-screw extruder, and the melt-blending conditions are: temperature 220°C and twin-screw extruder rotation speed 300 rpm; and the pellets are cut into pellets after traction and cooling to obtain a copolyester reinforced PET composite material.
[0090] Example 5
[0091] A method for preparing a PET composite material using waste PET and a pressure-sensitive adhesive tape comprises the following steps:
[0092] (1) The discarded pressure-sensitive adhesive tape 1 was melted at 260°C, stirred for 3.5 hours, and then an alcoholysis agent and a catalyst, tetrabutyl titanate, were added, and then vacuum polycondensed for 5 hours to obtain PET copolyester, wherein the amount of the alcoholysis agent was 150% of the mass of the pressure-sensitive adhesive tape. The amount of the catalyst was 0.5‰ of the mass of the discarded pressure-sensitive adhesive tape. The molecular weight of the prepared PET copolyester was determined to be about 27,000.
[0093] (2) 70 parts of waste PET (PET film with a number average molecular weight of about 40,000), 10 parts of talcum powder, 0.2 parts of dispersant TA100, and 0.2 parts of antioxidant 1010 are pre-mixed to obtain a pre-melt, and the pre-mixing conditions are: temperature 25°C, twin-screw extrusion, rotation speed of about 100 rpm, and pre-mixing time 3 minutes; 30 parts of the PET copolyester obtained in step (1) are melted at 260°C and kept warm for 5 minutes, and the molten PET copolyester is introduced from the die head and melt-blended and extruded with the pre-melt in a twin-screw extruder, and the melt-blending conditions are: temperature 220°C and twin-screw extruder rotation speed 300 rpm; after traction and cooling, the pellets are cut into pellets to obtain a copolyester reinforced PET composite material.
[0094] Example 6
[0095] A method for preparing a PET composite material using waste PET and a pressure-sensitive adhesive tape comprises the following steps:
[0096] (1) The waste pressure-sensitive adhesive tape 2 was melted at 260°C, stirred for 3 hours, and then an alcoholysis agent and a catalyst tetraisopropyl titanate were added, followed by vacuum polycondensation for 5 hours to obtain PET copolyester, wherein the amount of the alcoholysis agent was 150% of the mass of the pressure-sensitive adhesive tape and the amount of the catalyst was 0.5‰ of the mass of the waste pressure-sensitive adhesive tape; the molecular weight of the prepared PET copolyester was determined to be about 30,000.
[0097] (2) 80 parts of waste PET (PET film with a number average molecular weight of about 35,000), 15 parts of talcum powder, 0.5 parts of TA100, and 0.5 parts of antioxidant 168 are pre-mixed to obtain a pre-melt, and the pre-mixing conditions are: temperature 30°C, twin-screw extrusion, rotation speed of about 80 rpm, and pre-mixing time 3 to 10 minutes; 20 parts of the PET copolyester obtained in step (1) are melted at 260°C and kept warm for 10 minutes, and the molten PET copolyester is introduced from the die head and melt-blended and extruded with the pre-melt in a twin-screw extruder, and the melt-blending conditions are: temperature 230°C and twin-screw extruder rotation speed 200 rpm; and the pellets are cut into pellets after traction and cooling to obtain a copolyester reinforced PET composite material.
[0098] Example 7
[0099] A method for preparing a PET composite material using waste PET and a pressure-sensitive adhesive tape comprises the following steps:
[0100] (1) The waste pressure-sensitive adhesive tape 3 was melted at 265°C, stirred for 4 hours, and then an alcoholysis agent and a catalyst tetrabutyl titanate were added, followed by vacuum polycondensation for 5 hours to obtain PET copolyester, wherein the amount of the alcoholysis agent was 150% of the mass of the pressure-sensitive adhesive tape and the amount of the catalyst was 0.5‰ of the mass of the waste pressure-sensitive adhesive tape; the molecular weight of the prepared PET copolyester was determined to be about 34,000.
[0101] (2) 80 parts of waste PET (PET film with a number average molecular weight of about 45,000), 15 parts of talcum powder, 0.5 parts of dispersant TA100, and 0.5 parts of antioxidant 168 are premixed to obtain a premelt, and the premixing conditions are: temperature 20°C, twin-screw extrusion, rotation speed of about 200 rpm, and premixing time 4 minutes; 20 parts of the PET copolyester obtained in step (1) are melted at 265°C and kept warm for 5 minutes, and the molten PET copolyester is introduced from the die head and melt-blended and extruded with the premelt in a twin-screw extruder, and the melt-blending conditions are: temperature 210°C and twin-screw extruder rotation speed 400 rpm; and the pellets are cut into pellets after traction and cooling to obtain a copolyester reinforced PET composite material.
[0102] Example 8
[0103] A method for preparing a PET composite material using waste PET and a pressure-sensitive tape. This embodiment is substantially the same as Embodiment 1, except that the vacuum polycondensation time in this embodiment is 2 hours, and the molecular weight of the prepared PET copolyester is about 18,000.
[0104] Example 9
[0105] A PET composite material, this embodiment is substantially the same as embodiment 1, except that the molecular weight of the waste PET in this embodiment is about 20,000.
[0106] Comparative Example 1
[0107] A PET composite material, wherein comparative example 1 is substantially the same as example 1, except that the vacuum polycondensation time of comparative example 1 is 9 hours, and the molecular weight of the prepared PET copolyester is about 56,000.
[0108] Comparative Example 2
[0109] A kind of unmodified waste PET, wherein the waste PET is the same as the waste PET in Example 1.
[0110] The composite materials prepared in Examples 1 to 9 and Comparative Examples 1 to 2 were subjected to mechanical property tests, and the tensile, bending, and impact performance tests were all performed in accordance with GB / T 1040-2006, wherein the tensile rate of the tensile performance test was 50 mm / min.
[0111] The test results are shown in Table 1.
[0112] Table 1
[0113] Tensile strength / MPa Elongation at break / % Example 1 150.17 5.97 Example 2 152.68 4.79 Example 3 147.74 6.74 Example 4 153.47 4.21 Example 5 139.23 9.57 Example 6 147.28 6.86 Example 7 153.51 4.15 Example 8 134.52 7.84 Example 9 122.73 10.55 Comparative Example 1 156.17 3.16 Comparative Example 2 155.1 3.52
[0114] The glass transition temperature, melting point, crystallization temperature, etc. of the PET composite materials prepared in Examples 1-9 and Comparative Examples 1-2 were tested by differential thermal analysis, wherein the cold crystallization temperature test conditions were as follows: heating from room temperature to 280°C at a rate of 10°C / min, and keeping the temperature constant for 5 minutes; cooling from 280°C to 80°C at a rate of -5°C / min, and the sample slice weight was less than 10 mg. The test results are shown in Table 2.
[0115] Table 2
[0116]
[0117] The molecular weight of the PET copolyester in Comparative Example 1 is 56,000. Since its molecular weight is far more than 50,000, the carbonate in the PET copolyester with too large a molecular weight will form more intramolecular hydrogen bonds, causing greater polarity. At the same time, combined with a larger molecular weight, the cold crystallization temperature exceeds the cold crystallization temperature of conventional waste PET.
[0118] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the technical solution of the present invention, and are not intended to limit the specific implementation methods of the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the claims of the present invention shall be included in the protection scope of the claims of the present invention.
Claims
1. A PET composite material, characterized in that: The PET composite material comprises, by weight: 50-100 parts of PET, 5-30 parts of inorganic filler and 5-30 parts of PET copolyester; The PET copolyester is obtained by melting a waste pressure-sensitive adhesive product, adding an alcoholysis agent and a catalyst, and then polycondensing. The waste pressure-sensitive adhesive product includes a PET matrix and a pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer includes a copolyester elastomer. The copolyester elastomer is a copolymer of a carboxyl-terminated polyester and a non-crystalline carbon dioxide-based polyester diol. The number average molecular weight of the PET copolyester is less than 50,000.
2. The PET composite material according to claim 1, characterized in that: The 50 to 100 parts of PET include waste PET, wherein the polyester in the copolyester elastomer is polymerized by a C3-C7 dibasic acid and a C3-C7 diol, and the mass ratio of the polyester to the copolyester elastomer is 10 to 30 mass %, the number average molecular weight of the polyester is 1100 to 3000, the non-crystalline carbon dioxide-based polyester diol is a copolymer of polypropylene carbonate diol, and the number average molecular weight of the copolyester elastomer is 30000 to 50000.
3. The PET composite material according to claim 1, characterized in that: The PET composite material contains, by mass, 70 to 90 parts of the PET, and / or 10 to 20 parts of the inorganic filler, and / or 10 to 30 parts of the PET copolyester, and / or the cooling crystallization temperature of the PET composite material is 90 to 135° C., and / or the number average molecular weight of the PET copolyester is 15,000 to 50,000, and / or the tensile strength of the PET composite material is 120 to 160 MP, and / or the elongation at break of the PET composite material is 3% to 12%.
4. The PET composite material according to claim 3, characterized in that: The PET composite material also contains 0.2 to 1 parts of a dispersant, and / or 0.2 to 1 parts of an antioxidant, and / or the number average molecular weight of the PET copolyester is 20,000 to 50,000, and / or the molecular weight of the PET in the PET composite material is 35,000 to 45,000.
5. The PET composite material according to claim 1, characterized in that: The copolyester elastomer is a copolymer of polybutylene succinate and polypropylene carbonate diol, wherein the alcoholysis agent is one or more of methanol, ethanol, ethylene glycol, propylene glycol, butanediol and pentanediol, and the mass ratio of the alcoholysis agent to the pressure-sensitive adhesive product is (1-2):1; the catalyst is tetrabutyl titanate, tetraisopropyl titanate or p-toluenesulfonic acid, and the mass of the catalyst is 0.01-1% of the mass of the pressure-sensitive adhesive product; the pressure-sensitive adhesive product is a degradable tape, glue stick or film; the inorganic filler is one or more of talc, titanium dioxide, heavy calcium titanate, wollastonite, mica, kaolin, potassium titanate whisker, calcium carbonate whisker, barium sulfate and silicon dioxide.
6. The PET composite material according to claim 1, characterized in that: The pressure-sensitive adhesive layer in the waste pressure-sensitive adhesive product comprises, by parts by mass: 20-80 parts of copolyester elastomer; 20-50 parts of tackifying resin; 1 to 10 parts of plasticizer; and optional additives.
7. The PET composite material according to claim 6, characterized in that: The tackifying resin is one or more of natural rosin, hydrogenated rosin, disproportionated rosin, esterified rosin, C5 petroleum resin, C9 petroleum resin, and terpene resin; the plasticizer is one or more of epoxidized soybean oil, linseed oil, castor oil, and palm oil; the additive includes an antioxidant, and the antioxidant is one or more of tris(2,4-di-tert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, di(tridecanol)thiodipropionate, and tetrakis{3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate}pentaerythritol.
8. A method for preparing the PET composite material according to any one of claims 1 to 7, characterized in that: The steps include: (1) melting the waste pressure-sensitive adhesive product, adding an alcoholysis agent and a catalyst, and then polycondensing to obtain the PET copolyester; (2) Processing the components other than the PET copolyester into a premelt; adding the PET copolyester obtained in step (1) into the premelt, followed by melting, heat preservation, and extrusion to obtain the PET composite material.
9. The method for preparing the PET composite material according to claim 8, characterized in that: In step (1), the waste pressure-sensitive adhesive product is melted at 260-280° C., stirred for 3-4 hours, and after adding an alcoholysis agent and a catalyst, vacuum polycondensation is performed for 1-6.5 hours to obtain the PET copolyester.
10. The method for preparing the PET composite material according to claim 8, characterized in that: In step (2), the PET copolyester obtained in step (1) is introduced from the die head and melt-blended and extruded with the pre-melt. The melt-blending conditions are: temperature 200-240° C., and extruder speed of 100-500 rpm.
Citation Information
Patent Citations
Process for manufacturing non-woven fabric by waste PET (polyethylene terephthalate)
CN103374791A
Method for producing film sheet by direct melting of recovered waste PET (polyethylene terephthalate) andfilm sheet
CN106009545A
Recycled PET film manufactured using recycled chips
KR102611876B1
A process and an apparatus for manufacturing bi-axially oriented polyester film from rpet
US20220152904A1
Renewable pressure-sensitive adhesive and pressure-sensitive adhesive tape
CN110628361A