Anisotropic conductive adhesive and anisotropic conductive adhesive film connector using the same

By using thermosetting adhesives and conductive particles composed of polyphenoxy reactive resins and other components, an anisotropic conductive adhesive film with a high glass transition temperature and hydrophobicity is formed, which solves the problem of adhesion of acrylic thermosetting films in high temperature environments. and the problem of reduced conductivity, achieving stable conductivity and reliability on large-scale display panels.

CN118325487BActive Publication Date: 2024-10-29NANTONG DEJU SEMICON MATERIALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410760824.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-29
Estimated Expiration
2044-06-13

AI Technical Summary

Technical Problem

In high-temperature environments and high-humidity conditions, the adhesion and conductivity of acrylic thermosetting anisotropic conductive films decrease, and the grounding is insufficient, leading to reliability problems in display panels that are becoming larger and have improved image quality.

Method used

It uses thermosetting adhesive composed of polyphenoxy reactive resin, film-forming resin, thermoplastic rubber and polymerizable acrylic monomer, combined with conductive particles to form an anisotropic conductive adhesive film with high glass transition temperature and hydrophobicity. The stability and conductivity of the adhesive layer are ensured by means of heating and compaction tools.

Benefits of technology

It maintains adhesion and conductivity in high-temperature environments, offsets the bulging and peeling of the adhesive layer, ensures stable conductivity and reliability of circuit electrodes, and improves stability in high-temperature and high-humidity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118325487B_ABST
    Figure CN118325487B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of anisotropic conductive films, and specifically discloses anisotropic conductive adhesive and anisotropic conductive adhesive film connector using the adhesive. Thermosetting adhesive comprises the following components in proportion by weight: 5-40 parts of polyphenoxy reactive resin, 10-50 parts of film-forming resin, 10-40 parts of thermoplastic rubber, 5-35 parts of polymerizable acrylic monomer, and 1-5 parts of curing agent; wherein the average molecular weight of the polyphenoxy reactive resin is 1000g / mol-500000g / mol, the main chain of the polyphenoxy reactive resin is formed by linear polycondensation reaction of 2,6-xylenol at the 1st and 4th positions, respectively, and at least one end of the main chain is connected with OH or RCH2=CHCOO, and the film-forming resin is a resin with film-forming properties. In the present disclosure, when the polyphenoxyethylene having hydrophobic properties and a high glass transition temperature reaches a certain level, stable reliability can be ensured even in a high temperature environment and a high temperature and high humidity environment, thereby obtaining conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of anisotropic conductive films, and in particular relates to anisotropic conductive adhesive and anisotropic conductive adhesive film connector using the adhesive. Background Art

[0002] Anisotropic Conductive Film is used for electrical connection between flat panel displays such as LCD (liquid crystal display) and OLED (organic light emitting display) or semiconductor circuit boards and substrates.

[0003] Recently, as display panels have become larger and better in image quality, the electrodes in the circuit part have become thinner and thinner. In addition, in order to shorten the process time, the pressing time of the anisotropic conductive film has gradually shortened, and the original epoxy thermosetting film has been transferred to the acrylic thermosetting film. Therefore, under the harsh conditions of high temperature environment and high temperature and humidity environment, the anisotropic conductive film of the acrylic thermosetting component with slightly fragile thermal stability has the problem of decreased adhesion and conductivity, and insufficient grounding. Summary of the invention

[0004] In order to solve the above problems, the present invention provides the following solutions:

[0005] The first aspect of the present invention relates to a thermosetting adhesive comprising the following components in parts by weight:

[0006] 5-40 parts of polyphenoxy reactive resin, 10-50 parts of film-forming resin, 10-40 parts of thermoplastic rubber, 5-35 parts of polymerizable acrylic monomer, and 1-5 parts of curing agent; wherein,

[0007] The average molecular weight of the polyphenoxy reactive resin is 1000 g / mol to 500000 g / mol. The main chain of the polyphenoxy reactive resin is formed by linear polycondensation of 2,6-xylenol at the 1st and 4th positions (as shown below), and at least one end of the main chain formed by the reaction is connected with -OH or RCH2=CHCOO-, where R is H- or alkyl.

[0008]

[0009] The film-forming resin is a resin having film-forming properties.

[0010] As for the allocation ratio of each group, it can be further as follows: in a further scheme, the specific content of each component is:

[0011] 1) 10-35 parts of polyphenoxy reactive resin,

[0012] 2) 15~30 parts of thermoplastic rubber,

[0013] 3) 10~25 parts of polymerizable acrylic acid monomer,

[0014] 4) 1.5~3 parts of curing agent.

[0015] For each of the above characteristics, any of the following conditional characteristics may be further selected:

[0016] One of them, the polyphenoxy reactive resin is at least any one of the compounds represented by Formula I to Formula IV, wherein: n and m are both positive integers,

[0017] ,

[0018] The corresponding polymer can adopt the existing scheme, for example, the products in Formula III and Formula IV can be SABIC's NORYL™ SA90 resin; further introduced, the load deformation temperature of polyphenoxy reactive resin can reach above 190°C, and the molding temperature is -170°C, which can ensure stable reliability characteristics in high temperature environment or high temperature and high humidity environment;

[0019] Second, the film-forming resin is at least any one of phenol resin, unsaturated polyester resin, saturated polyester resin, polyurethane resin, butadiene resin, polyimide resin, polyimide resin, polyolefin resin, and polystyrene resin. Preferably, the average molecular weight of the film-forming resin is 10,000 to 80,000;

[0020] Three of them, the thermoplastic rubber is at least one of silicone rubber, nitrile rubber, polyisoprene rubber, polybutadiene rubber, carboxyl-terminated polybutadiene rubber, hydroxyl-terminated polybutadiene rubber, 1,2-polybutadiene rubber, carboxyl-terminated 1,2-polybutadiene rubber, hydroxyl-terminated 1,2-polybutadiene rubber, styrene-butadiene rubber, hydroxyl-terminated styrene-butadiene rubber nitrile rubber, acrylonitrile-butadiene rubber, carboxylated nitrile rubber, hydroxyl-terminated poly(oxypropylene) rubber, alkoxysilyl-terminated poly(oxypropylene) rubber, poly(oxytetramethoxy) glycol rubber, polyolefin glycol rubber and poly-ε-caprolactone thermoplastic rubber, preferably chloroprene rubber thermoplastic rubber;

[0021] Four of them, the polymerizable acrylic monomer is at least one of ethylene glycol diacrylate, phosphate ester acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, acrylonitrile, 4-hydroxybutyronitrile, isobutyronitrile, t-butyronitrile, isooctyl acrylate, non-ferrite ethanol fluoroacrylate, 2-propylene monooxyethyl ester succinic acid, dodecanitrile, octadecene acrylate, isobutyl acrylate, trichlorocandimethyl alcohol diacrylate, trichlorohexasilyl acrylate, triS (2-hydroxyethyl) isocyanate triacrylate, tetrahydrofuran acrylate, o-phthalic acid diester ether acrylate, ethoxylated bisphenol A dicarboxylate, bisphenol A type epoxy acrylate, polyurethane acrylate, epoxy acrylate;

[0022] In five of them, the curing agent is at least one of hydroxymethyl cyclohexanone, dialkyl cyclohexanone, peroxide ester, dimethylene cyclohexanone, keto cyclohexanone, peroxide carbonate, and peroxide ketone; preferably, the curing agent is at least t-butyl terephthalic acid, 1,1,3,3-tetramethyl terephthalic acid-2-ethylhexanoic acid, 2,5-dimethyl-2,5-di(2-ethylhexanoic acid)hexanoic acid, 1-cyclohexyl-1-methyl-2-ethylhexanoic acid, 2,5-dimethyl-2-butylhexanoic acid, 1-propyl hexanoic acid, 1-butyl hexanoic acid, 1-propyl ester, 1-butyl hexanoic acid, 1-butyl Adipic acid, 1-propyl 2-ethylhexyl monocarbonate, t-hexyl hexyl benzoate, t-butyl hexyl hexanoate, D-butyl hexanoate, 2,5,-dimethyl-2,5-di(t-butylperoxy)hexane, t-butyl hexanoate, t-hexyl hexanoate-2-butyl hexanoate, 2-2-butyl hexanoate Tirate, 1,1-di(t-butyloxy)cyclohexane, t-hexyloxyisopropofol monobarbonate, t-butyloxy-3,5,5-trimethoxyhexane, t-butyloxyvalerate, Kumilperoxinodecanoate, diisopropylbenzyloxybenzoate Benzyl, quinoline hydroxybenzyloxy, isobutylbenzyloxy, 2,4-dichlorobenzyloxy, 3,5,5-trimethoxybenzyloxy, tert-octylbenzyloxy, benzyloxy, 3,5-trimethoxybenzyloxybenzyloxy, benzyloxybenzyloxy, ketone oxide, 1,1,3,3-tetramethylbutadienyloxysuccinate, 1-dichlorohexyl-1-methylethyl hydroxyethyl carbonate, Dn-propoxy carbonate, diisopropyl carbonate, bis(4-t-butylcyclohexyl) peroxydicarbonate, di-2-dipropyl adipate, di(2-ethyladipate)dipropyl adipate Levonite, dimethoxy Benzoate, bis(3-methyl-3-methoxybenzoate) dimethicone, 1,1-vis(t-cyclodextrin)-3,3,5-trimethylcyclohexane, 1,1-dioxadi ...

[0023] In the above, at least means that at least this group can be selected, but it is not limited to this, and there may be other options.

[0024] The second aspect of the present invention relates to a conductive adhesive, comprising the aforementioned thermosetting adhesive and conductive particles mixed therewith;

[0025] The allocation ratio of each group is

[0026] 5-40wt% polyphenoxy reactive resin, 10-50wt% film-forming resin, 10-40wt% thermoplastic rubber, 5-35wt% polymerizable acrylic monomer, 1-5wt% curing agent, 1-10wt% conductive particles, and the remainder are auxiliary materials. Auxiliary materials are not necessary, and can be some conventional additives or "zero" auxiliary materials.

[0027] For each of the above characteristics, any of the following conditional characteristics may be further selected:

[0028] One of them, the particles mentioned can further adopt the following scheme, and at least one of them can be selected,

[0029] 1) The conductive particles are metal particles or carbon-based particles;

[0030] 2) The carbon-based particles are at least one of carbon-containing polystyrene, polyester, polyethylene, benzoimide and polyol;

[0031] 3) The metal particles are at least one of Au, Ag, Ni, Cu-Pb, Al, Cr, Sn, Ti, and Pb.

[0032] In another embodiment, the outer diameter of the conductive particles is 0.1-30 μm; further, the outer diameter of the conductive particles is 0.2-15 μm.

[0033] Among them, the specific content of any one of the components is, and at least one of them can be selected, and when any one is selected, the rest can be set according to the above ratio,

[0034] 1) Polyphenoxy reactive resin 10~35wt%,

[0035] 2) Thermoplastic rubber 15~30wt%,

[0036] 3) Polymerizable acrylic acid monomer 10~25wt%,

[0037] 4) Curing agent 1.5~3wt%.

[0038] The third aspect of the present invention relates to a conductive film, comprising a substrate and the conductive adhesive disposed on the substrate. Figure 1 As shown in , a layered structure is formed by mixing a thermosetting adhesive and conductive particles, and finally forming an anisotropic conductive adhesive film loaded with a conductive filler; and the substrate is as Figure 1 As shown in , it can be a polyethylene tetrabenzoate film.

[0039] For each of the above characteristics, any of the following conditional characteristics may be further selected:

[0040] In one of the methods, the conductive adhesive tape is placed on the substrate and then dried in an environment of 60-130° C. for 30-300 seconds.

[0041] In one of the above, the substrate is at least one of a polyethylene glycol ester film, a polyimide film, and a polyethylene tetrabenzoate film; preferably, the substrate is pre-treated with silicon or fluorine, and the thickness of the substrate is 20-100 μm.

[0042] Among them, the conductive film can be used in specific applications. Figure 2 As shown in: the connection structure using conductive film can be such as ground circuit substrate, flexible wiring substrate (substrate), etc.; the terminal of the substrate can be a gasket electrode, wire electrode, pump electrode, etc. formed by electrode materials such as copper, aluminum, Ag, Au, ITO, etc.; when using, the thermosetting adhesive is pressed on these substrates, and then connected to functional modules such as ICchip, LCD panel, OLED panel, IC module, etc., and the terminal of the functional module (such as display module) can be a gasket electrode, wire electrode, pump electrode, etc. formed by electrode materials such as copper, aluminum, Ag, Au, ITO, etc. More specifically, the electrodes of two oppositely arranged electronic components can be opposite to each other, and a thermosetting adhesive composition (thermosetting adhesive) can be arranged between them, and heated by a heating and pressing compacting tool, and the adhesive layer is heated at the same time. While heating, wait for the composition to soften or melt, and continue heating after starting heating. It is best to harden the adhesive layer for more than 2 seconds to about 10 seconds.

[0043] In the solution provided by the present disclosure, when the polyphenylene oxide having a hydrophobic property and a high glass transition temperature reaches a certain level, stable reliability can be ensured even in a high temperature environment and a high temperature and high humidity environment, thereby obtaining conductivity. After a certain ratio of polyphenylene oxide is cured, due to the characteristics of high glass transition temperature and hydrophobicity, the bulge and peeling of the adhesive layer are offset in a high temperature environment or a high temperature and high humidity environment, thereby obtaining stable conductivity of the circuit electrode part of the conductive filler on the resin. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 It is one of the examples of anisotropic conductive film;

[0045] Figure 2 This is one of the examples of connection using different conductive films;

[0046] Figure 3 The following are the configuration schemes and performance test results for each instance.

[0047] In the figure:

[0048] 10 anisotropic conductive adhesive film, 20 conductive filler, 30 polyethylene tetrabenzoate film, 40 ITO Glass, 50 polyimide film, 60 first metal electrode, 70 second metal electrode. DETAILED DESCRIPTION

[0049] Hereinafter, the present invention will be specifically described by way of examples.

[0050] <Example Conductive Thin Film Formation Scheme>

[0051] The non-conductive adhesive composition obtained by mixing the formulation components shown in Table 1 in a conventional manner was coated on a shaped polyester (PET) film and dried at 80° C. for 120 seconds to obtain an adhesive film with a thickness of 25 μm.

[0052] (Implementation Example 1)

[0053] A polyphenoxy ester resin (manufactured by SABIC, trade name: SA-9000) is 10 parts by weight, a bisphenol A type epoxy phenol resin (manufactured by Nippon Steel Chemical, trade name: YP-50S) is 40 parts by weight, a thermoplastic acrylonitrile rubber (manufactured by Zeon Chemical, trade name: Nipol1072CGJ) is 25 parts by weight, and an acrylonitrile single composition (manufactured by Miwon Chemical, trade name: Mira0M) is 1140F, trade name: NIPER weight part (NOT) is 15 parts by weight) The composition was prepared by uniformly mixing 1.5 parts by weight of isooctyloxy ester (manufactured by NOF, trade name: PERHEXA250) and 3 parts by weight of conductive particles (manufactured by Duksan Neolux, trade name: PGL-B5.5R) by a conventional method.

[0054] (Implementation Example 2)

[0055] With respect to Example 1, except for changing to the configuration shown in Table 1, an anisotropic conductive film was prepared in the same manner as Example 1.

[0056] (Implementation Example 3)

[0057] With respect to Example 1, except for changing to the configuration shown in Table 1, an anisotropic conductive film was prepared in the same manner as Example 1.

[0058] (Implementation Example 4)

[0059] With respect to Example 1, except for changing to the configuration shown in Table 1, an anisotropic conductive film was prepared in the same manner as Example 1.

[0060] (Implementation Example 5)

[0061] With respect to Example 1, except for changing to the configuration shown in Table 1, an anisotropic conductive film was prepared in the same manner as Example 1.

[0062] (Implementation Example 6)

[0063] With respect to Example 1, except for changing to the configuration shown in Table 1, an anisotropic conductive film was prepared in the same manner as Example 1.

[0064] (Comparative Example 1)

[0065] Compared with Example 1, except that the polyphenylene oxide resin was replaced by comparative polyurethane acrylate, an anisotropic conductive film was prepared in the same manner as Example 1 except that the configuration was changed to that shown in Table 1.

[0066] (Comparative Example 2)

[0067] With respect to Comparative Example 1, except that the configuration was changed to that shown in Table 1, the same procedures as in Example 1 were followed to prepare an anisotropic conductive film.

[0068] (Comparative Example 3)

[0069] With respect to Comparative Example 1, except that the configuration was changed to that shown in Table 1, the same procedures as in Example 1 were followed to prepare an anisotropic conductive film.

[0070] (Comparative Example 4)

[0071] With respect to Comparative Example 1, except that the configuration was changed to that shown in Table 1, the same procedures as in Example 1 were followed to prepare an anisotropic conductive film.

[0072] (Comparative Example 5)

[0073] With respect to Comparative Example 1, except that the configuration was changed to that shown in Table 1, the same procedures as in Example 1 were followed to prepare an anisotropic conductive film.

[0074] (Comparative Example 6)

[0075] With respect to Comparative Example 1, except that the configuration was changed to that shown in Table 1, the same procedures as in Example 1 were followed to prepare an anisotropic conductive film.

[0076] <Production of Chimeras and Evaluation of Chimeras>

[0077] Chimeras were prepared according to the following method and the following evaluations were performed. The results are shown in Table 1.

[0078] The adhesive used for the adhesion test is a glass substrate, and an ITO wiring board with an average thickness of 0.7mm is used, inlaid with an ITO (Indium Tin Oxide) film. The glass substrate is 50mm wide by 30mm wide, and a 1.2mm width of a different conductive film is pressed on it. After fixing the flexible wiring substrate (18 micron thick copper on polyimide with gold-coated electrodes, Pitch 150 micron) representing the conductive film after pressure, as a buffer material, a 200 micron thick silicone rubber sheet is sandwiched, and the bonding is completed using a thermal tool at 170°C, 3Mpa, and 7sec. The completed chimera is used for adhesion evaluation and connection resistance evaluation.

[0079] <Adhesion Evaluation>

[0080] The adhesive strength of the manufactured bonded body was evaluated using a universal testing machine (model: Sur TA1Ae, CHEMILAB) with a measurement width of 10 mm and a 90° Peel test. The values ​​at the initial stage, 100°C / 500 hours, and 85°C-85%RH / 500 hours were measured at a tool speed of 50 mm / min. The results were evaluated according to the following evaluation criteria. The results are shown in Table 1.

[0081] Evaluation criteria: ○: 900 gf / cm or more; △: 600-900 gf / cm or less; X: 600 gf / cm or less.

[0082] <Connection resistance evaluation>

[0083] The connection resistance of the manufactured chimera was evaluated by measuring the connection resistance at 1 mA using the four-stage method, and the values ​​after the initial stage, 100°C / 500 hours, and 85°C-85%RH / 500 hours were evaluated according to the following evaluation criteria. The results are shown in Table 1.

[0084] Evaluation criteria: ○: less than 0.3; △: less than 0.3-0.6; X: 0.6 or higher.

[0085] <Evaluation of moisture absorption rate>

[0086] Thermosetting films were stacked into sheets with a width of 50 mm, a width of 50 mm, and a thickness of 0.2 mm. After being made into seats, they were completely cured at 170°C for 5 minutes, and then placed in a beaker filled with pure water for 24 hours. The weight difference before and after was measured and evaluated according to the following evaluation criteria. At this time, the water temperature was fixed at 25°C. The results are shown in Table 1. The moisture absorption rate is calculated as follows (1).

[0087] Moisture absorption rate (%) = W1-W0 / W0× 100 Formula (1)

[0088] W0: initial sample weight, W1: sample weight after moisture absorption

[0089] Evaluation criteria: ○: less than 0.2%, △: 0.2% to 0.5% or less, X: 0.5% or more.

[0090] The units of the proportions shown in Table 1 are parts by weight.

[0091] SA-9000: bifunctional polystyrene oxide acrylate resin, manufactured by SABIC; UA-2374 PIB: polyurethane acrylate, manufactured by Shin-Nakamura chemical; YP-50S: bisphenol A epoxy phenolic resin, manufactured by Nippon steelchemical; Nipol1072CGJ: acrylonitrile rubber, manufactured by Zeon Chemical; Miramer M1140: isobutyl acrylate, manufactured by Miwon special chemical; Nyper BMT: Yashirper Osside, manufactured by NOF;

[0092] PERHEXA 250: Oxygen-enriched ester, manufactured by NOF; PGL-B5.5R: Conductive particles, manufactured by Duksan neolux.

[0093] <Inspection of the results of Table 1>

[0094] It has been confirmed that the reliability stability of the conductive film containing polyphenylene oxide in high temperature environment and high temperature and high humidity environment at different mass ratios is better than that of the commonly used polyurethane acrylate. It can be seen that when the content of polyaniline is 10% by weight and 35% by weight, the stability in high temperature and high humidity environment decreases, but when the content is appropriate, 10 to 30% by weight, good reliability stability can be ensured.

[0095] On the contrary, the urethane acrylate of the comparative example of the different conductive films generally showed decreased adhesion and connection resistance in the initial comparative high temperature environment and the high temperature and high humidity environment, and the reliability stability decreased.

[0096] In addition, the moisture absorption results show that the moisture absorption of the anisotropic conductive film containing polyphenoxy is excellent, so it is believed that its barrier property to water is also very good. However, in comparison, the barrier property of polyurethane acrylate is generally inferior to that of polyphenoxy.

[0097] Based on the results, it can be concluded that polyphenylene oxide is easy to react radially with organic peroxides, and the physical properties it follows also meet the requirements of anisotropic conductive films. Its main characteristics are high glass transition temperature and hydrophobicity. It can be confirmed that it has good reliability and stability in high temperature environments and high temperature and high humidity environments of anisotropic conductive films.

[0098] <Industrial Usability>

[0099] The limitations of the currently commonly used polyurethane acrylates are the design with high glass transition temperature and hydrophobic properties. In order to improve this, many additives can only be used in the components of the non-conductive adhesive composition. Therefore, the process becomes complicated and the distribution of quality is difficult to be uniform. In addition, as the cost composition ratio of additional material input increases, it will become disadvantageous to produce economical products. As mentioned above, polyphenylene oxide shows excellent characteristics in ensuring more stable reliability than polyurethane acrylate. Therefore, if the proportion is appropriately adjusted in the heteroconductive adhesive composition for design, it will help to ensure stable reliability in high temperature environment and high temperature and high humidity environment.

[0100] It is clear to those skilled in the art that various modifications to the above embodiments can be made without departing from the overall spirit and concept of the present invention, and matters not detailed in the present disclosure can refer to the prior art. They all fall within the scope of protection of the present invention. The protection scheme of the present invention shall be subject to the claims attached to the present invention.

Claims

1. Conductive film, characterized in that: It includes a substrate and a conductive adhesive arranged on the substrate; wherein the conductive adhesive includes a thermosetting adhesive and conductive particles mixed therewith; wherein the proportion of each component is: 10-35wt% polyphenoxy reactive resin, 10-50wt% film-forming resin, 15-30wt% thermoplastic rubber, 10-25wt% polymerizable acrylic monomer, 1.5-3wt% curing agent, 1-10wt% conductive particles, and the remainder as auxiliary materials; in, The average molecular weight of the polyphenoxy reactive resin is 1000 g / mol to 500000 g / mol. The polyphenoxy reactive resin is any one of the compounds represented by Formula I to Formula IV, wherein n and m are both positive integers. The compound of formula III is NORYL from SABIC TM SA90 resin, Formula IV is NORYL of SABIC TM SA9000 resin; After the conductive tape is placed on the substrate, it is dried in an environment of 60 to 130° C. for 30 to 300 seconds. The substrate is any one of a polyethylene glycol ester film and a polyimide film. The substrate is pre-treated with silicon and fluorine, and the thickness of the substrate is 20 to 100 μm. The conductive particles have an outer diameter of 0.1 to 30 μm.

2. The conductive film according to claim 1, characterized in that: The film-forming resin is any one of phenol resin, unsaturated polyester resin, saturated polyester resin, polyurethane resin, butadiene resin, polyimide resin and polyolefin resin; The thermoplastic rubber is at least one of silicone rubber, nitrile rubber, polyisoprene rubber and chloroprene rubber; The polymerizable acrylic monomer is at least one of ethylene glycol diacrylate, phosphate ester acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, acrylonitrile, isooctyl acrylate, isobutyl acrylate, tetrahydrofuran acrylate, polyurethane acrylate, and epoxy acrylate; The curing agent is at least one of hydroxymethylcyclohexanone, dialkylcyclohexanone, peroxide ester, ketocyclohexanone, peroxide carbonate and peroxide ketone.

3. The conductive film according to claim 2, characterized in that: The average molecular weight of the film-forming resin is 10,000 to 80,000.

4. The conductive film according to claim 1, characterized in that: The conductive particles are metal particles or carbon-based particles; The carbon-based particles are at least one of carbon-containing polystyrene, polyester, polyethylene, benzimide and polyol. The metal particles are at least one of Au, Ag, Ni, Cu-Pb, Al, Cr, Sn, Ti, and Pb.

5. The conductive film according to claim 1, characterized in that: The conductive particles have an outer diameter of 0.2 to 15 μm.

Citation Information

Patent Citations

  • Acrylic composition for sealing, sheet material, multilayer sheet, cured product, semiconductor device and method for manufacturing semiconductor device

    CN109564903A