A recombinant collagen composite gel, dressing and application thereof
By combining recombinant collagen with polyamino acids and biological cross-linking agents, the viscosity and biocompatibility problems of hydrogel products are solved, forming a gel with high biocompatibility and moderate viscosity, which significantly improves wound healing. effect and reduce toxicity.
Patent Information
- Application Number
- CN202410778423.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-17
AI Technical Summary
Existing hydrogel products face problems such as too high or too low viscosity, poor air permeability, and low moisture content, which affect the wound healing effect. In addition, traditional chemical cross-linking agents are highly toxic and have poor biocompatibility.
It uses recombinant collagen composite gel, which contains recombinant collagen, polyamino acids, biological cross-linking agents and metal chlorides. It is cross-linked by glutamine transaminase or glutamyl endopeptidase to form a high biocompatibility and moderate viscosity of gel, increasing the mechanical stability and breathability of the gel.
It significantly improves the wound healing speed, increases cell vitality, reduces toxicity, ensures the high biocompatibility and good skin-friendly properties of the gel, and avoids the problem of viscosity decrease after radiation sterilization.
Smart Images

Figure CN118340935B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of dressings, and in particular to a recombinant collagen composite gel, a dressing and applications thereof. Background Art
[0002] Hydrogels are formed by water-soluble or hydrophilic polymers through certain chemical or physical cross-linking. Among them, hydrogels prepared from natural polymers have the advantages of biocompatibility, biodegradability, and a microenvironment similar to natural tissues. At present, the natural polymer materials used to prepare hydrogels are mainly animal collagen and sodium hyaluronate. Collagen is a biopolymer and the most abundant and widely distributed functional protein in mammals, accounting for 25-30% of the total protein.
[0003] At present, the prior art generally adopts two methods for cross-linking hydrogels: physical cross-linking and chemical cross-linking. Physically cross-linked hydrogels are formed by physical forces such as electrostatic effects and hydrogen bonds. During the preparation process, there is no need to use cross-linking agents that are toxic to cells or affect the activity of biological molecules, but their stability is poor and their strength is low. The hydrogels prepared by chemical cross-linking have better stability and higher flexibility. However, since chemical cross-linking agents such as 1,4-butanediol diglycidyl ether and sodium β-glycerophosphate need to be used during the cross-linking process, the toxicity is high, and if the residual is not completely removed, it will cause damage to the human body. Prior art CN115400260A discloses a repair gel containing recombinant humanized collagen and a preparation method thereof, using disodium ethylenediaminetetraacetic acid as a coupling agent. The method also uses a chemical cross-linking method to prepare the gel.
[0004] However, the relevant gel products on the market face problems such as high viscosity, low viscosity, poor air permeability or low water content, which may affect the use effect of the product. Dressings with excessive viscosity will hinder the contact between the wound and the air, affect the respiration and metabolism of cells, and thus affect the healing speed of the wound. When changing materials, they may cause damage to the skin and increase the risk of infection. On the other hand, low-viscosity dressings may not provide sufficient support and protection. Dressings with poor air permeability may cause the wound to be sealed and airtight, prone to suppuration, and not conducive to the normal healing of the wound. Low water content can cause local dryness and may also cause dehydration of tissues around the wound, further aggravating skin damage. Despite this, the current technology has not yet conducted in-depth research on the comfort of gel use. CN115804864A discloses a synergistic repair-promoting heat-stable recombinant type III humanized collagen gel and a preparation method thereof. The gel uses carbomer and trehalose to interact with collagen for cross-linking to form a three-layer structure, and the gel viscosity can reach up to 100,000 mPa·s. In addition, the patent document also mentioned that excessive gel viscosity may affect the solvation of collagen. In the actual production process, recombinant collagen gel is usually used after radiation sterilization, while the viscosity of the gel after simple carbomer resin cross-linking will decrease to varying degrees after radiation sterilization.
[0005] In order to solve these problems, it is necessary for us to conduct in-depth investigation and research on the comfort of gel use, and to carry out research and development and adjustments from the aspects of raw material formula, preparation method, performance testing, effect testing, etc., in order to solve a series of problems with existing products and methods. Summary of the invention
[0006] The present invention overcomes the defects of the prior art gel raw materials, such as poor biocompatibility, high toxicity, too high / low viscosity or low water content of gel products, thereby providing a recombinant collagen composite polyamino acid gel. The recombinant collagen composite gel and dressing products prepared by the present invention have milder ingredients, moderate viscosity, simple and feasible raw materials and methods while ensuring excellent repair effects.
[0007] The present invention solves the above technical problems through the following technical solutions.
[0008] The present invention provides a recombinant collagen composite gel, which comprises the following preparation raw materials: 0.1-0.5wt% of recombinant collagen, 3-10wt% of polyamino acid, 0.1-0.4wt% of biological cross-linking agent and 1-5wt% of metal chloride;
[0009] The recombinant collagen is at least one of recombinant type III human collagen and recombinant type IV human collagen;
[0010] The biological cross-linking agent is transglutaminase or glutamyl endopeptidase.
[0011] The biocrosslinking agents of the present invention are safe and non-toxic. They can efficiently catalyze the crosslinking process of recombinant collagen, enhance the interaction between gel and cells, significantly improve its biocompatibility, and further help promote the repair and regeneration of skin tissue.
[0012] In the present invention, the biological cross-linking agent is transglutaminase.
[0013] In the present invention, the biological cross-linking agent is glutamyl endopeptidase.
[0014] In the present invention, the recombinant collagen composite gel comprises the following preparation raw materials: 0.15-0.45wt% of recombinant collagen, 4-8wt% of polyamino acid, 0.1-0.2wt% of biological cross-linking agent and 2-3wt% of metal chloride.
[0015] The optional values of the amount of recombinant collagen used are 0.1wt%, 0.15wt%, 0.2wt% or 0.3wt%, 0.4wt%, 0.45wt%, 0.5wt%.
[0016] The optional values of the amount of polyamino acid used are 3wt%, 4wt%, 5wt%, 6wt% or 8wt%.
[0017] The optional value of the amount of the bio-crosslinking agent is 0.1wt%.
[0018] The optional value of the amount of metal chloride is 2.0wt% or 2.5wt%.
[0019] In the present invention, the polyamino acid is at least one of polylysine, polyglutamic acid, polyvaline, polyleucine, polyaspartic acid, polythreonine and polycysteine. The polyamino acid material itself has excellent biocompatibility and biodegradability. In addition, the polyamino acid in the gel of the present invention also has the advantages of providing viscosity and water retention, and enhancing the mechanical stability of the gel, which is very important for promoting wound healing.
[0020] In the present invention, the metal chloride is at least one of sodium chloride, potassium chloride and zinc chloride. Among them, the metal chloride can play a pore-forming role, and appropriate addition can make the gel have a porous structure; therefore, the gel will become more comfortable, soft and breathable; on the other hand, the metal chloride will affect the activity of the biocrosslinking agent, so the addition of the pore-forming agent needs to be controlled within the above-mentioned dosage range to make the gel take into account both comfort and efficacy.
[0021] In the present invention, the recombinant collagen is recombinant type III human collagen.
[0022] In the present invention, the molecular weight of the recombinant type III human collagen is 35-60KD.
[0023] In the present invention, the molecular weight of the recombinant type IV human collagen is 150-200 KD.
[0024] In the present invention, the molecular weight of the polyamino acid is 3800-1100000.
[0025] In the present invention, the molecular weight of the polylysine is 3800-4300.
[0026] In the present invention, the molecular weight of the polyglutamic acid is 700,000-1,100,000.
[0027] In the present invention, the molecular weight of the polyvaline is 30,000-70,000.
[0028] In the present invention, the molecular weight of the polyleucine is 40,000-60,000.
[0029] In the present invention, the molecular weight of the polyaspartic acid is 6000-8000.
[0030] In the present invention, the molecular weight of the polythreonine is 8000-10000.
[0031] In the present invention, the molecular weight of the polycysteine is 10,000-20,000.
[0032] Among them, the molecular weight of polyamino acids will affect its hydrophilicity and hydrophobicity and the interaction with other molecules, thereby affecting the overall performance of the gel. Therefore, in order to meet the needs, it is necessary to select a suitable molecular weight of polyamino acids, which can optimize the biocompatibility of the gel and promote cell adhesion, thereby improving the therapeutic effect.
[0033] In the present invention, the recombinant collagen composite gel further contains carbomer.
[0034] Furthermore, the carbomer is at least one of carbomer 941, carbomer 971, carbomer 981, carbomer U20 and carbomer 2020.
[0035] In the present invention, the recombinant collagen composite gel further contains a moisturizer and a preservative.
[0036] Furthermore, the moisturizing agent is glycerin, propylene glycol or sodium hyaluronate.
[0037] Furthermore, the preservative is at least one of methylparaben (CAS No.: 99-76-3) and phenoxyethanol (CAS No.: 122-99-6).
[0038] In the present invention, the recombinant collagen composite gel is composed of the following preparation raw materials:
[0039] Recombinant collagen 0.1-0.5wt%, polyamino acid 3-10wt%, carbomer 0.3-1wt%, metal chloride 1-5wt%, biocrosslinking agent 0.1-0.4wt%, preservative 0.1-0.9wt%, humectant 1-6wt% and balance water.
[0040] Preferably, the raw materials for preparing the recombinant collagen composite gel further include: 0.5-0.7wt% of carbomer; more preferably, the optional value of the amount of carbomer is 0.5wt% or 0.7wt%.
[0041] Preferably, the raw materials for preparing the recombinant collagen composite gel further include: 3-4wt% of a moisturizer; more preferably, the optional value of the amount of the moisturizer is 3wt% or 4wt%.
[0042] Preferably, the raw materials for preparing the recombinant collagen composite gel further include: 0.1-0.6wt% of preservative; more preferably, the optional value of the amount of preservative is 0.1wt%, 0.5wt% or 0.6wt%.
[0043] The recombinant collagen composite gel as mentioned above is prepared by mixing the preparation raw materials.
[0044] The present invention provides a recombinant collagen composite dressing comprising the recombinant collagen composite gel as described above.
[0045] A method for preparing a recombinant collagen composite dressing comprises the steps of filtering the recombinant collagen composite gel as described above and injecting it into a sheet-shaped molding mold, rapidly freezing it to obtain a frozen dressing product, and then drying and demolding the frozen dressing product to obtain the recombinant collagen composite dressing. Preferably, the mold is a sheet-shaped mold.
[0046] The aforementioned recombinant collagen composite gel, or the aforementioned recombinant collagen composite dressing, is used in the preparation of a product for treating non-chronic wounds and / or skin inflammation. The non-chronic wounds include superficial wounds, postoperative suture wounds, mechanical trauma, small wounds, abrasions, cut wounds, puncture sites of puncture instruments, first degree or shallow second degree burn wounds, and postoperative wounds of laser / photon / acid peeling / micro-plastic surgery. The skin inflammation includes acne vulgaris, dermatitis, and sensitive skin.
[0047] The recombinant collagen composite gel and dressing prepared by the present invention are stored at room temperature in a dry, ventilated environment without corrosive gases; during transportation, they should be protected from heavy pressure, direct sunlight, rain and snow.
[0048] The recombinant collagen composite gel and dressing may also be sterilized before packaging, and the sterilization is performed by cobalt 60 irradiation sterilization or electron beam irradiation sterilization. Furthermore, the irradiation dose of the cobalt 60 irradiation sterilization is 15 to 30 kGy; the irradiation dose of the electron beam irradiation sterilization is 15 to 30 kGy.
[0049] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0050] Compared with the prior art, the present invention has the following beneficial effects:
[0051] 1. The raw materials of the present invention are appropriately selected and the synergistic effect of the formula is remarkable:
[0052] Recombinant (human) collagen provides good biocompatibility and functionality, polyamino acids enhance the mechanical properties and stability of the gel, and biocrosslinkers provide the gel with bioactive components; these two raw materials have significant synergistic effects with the recombinant human collagen formula.
[0053] 2. Rapidly repair wounds with remarkable results:
[0054] Animal experiments on wound repair show that wounds treated with this product heal better than untreated wounds, with significantly faster wound recovery, no purulent tissue, and no new granulation tissue. In addition, the efficacy of the dressing combined with LED irradiation in treating facial dermatitis reached 90.39%.
[0055] 3. Low product toxicity:
[0056] The recombinant collagen composite gel of the present invention has extremely low toxicity, and cells cultured in the gel extract still have high cell viability after 1 day, 3 days and 5 days, so its cytotoxicity is classified as level 0. This is due to the natural, safe and highly biocompatible raw materials selected, which is beneficial to cell viability and promotes cell growth.
[0057] 4. Gel and dressing products have excellent performance:
[0058] The product has moderate shear viscosity (22~30Pa·s), high water retention rate (82~92%), good air permeability, good lubricity (friction coefficient is only 0.11~0.17), so it has better skin affinity. In addition, the viscosity of this product remains even after irradiation sterilization, and there will be no problem of product viscosity reduction. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] Figure 1 This is a real picture of the recombinant collagen composite gel sample.
[0060] Figure 2 Schematic diagram of the preparation of recombinant collagen composite gel.
[0061] Figure 3 This is a scanning electron micrograph of the gel prepared in Examples 1 to 4.
[0062] Figure 4 The following are scanning electron micrographs of the gels prepared in Example 1 and Comparative Example 1.
[0063] Figure 5 Image of full-thickness skin defect repair in wound repair animal experiment. DETAILED DESCRIPTION
[0064] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and carefully in combination with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.
[0065] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0066] "Scope" disclosed in the present invention is defined in the form of lower limit and upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a particular range. The scope defined in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a particular parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3,4 and 5 are listed, the following scope can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present invention, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0067] If not otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form a new technical solution.
[0068] Unless otherwise specified, all technical features and optional technical features of the present invention can be combined with each other to form a new technical solution.
[0069] If not otherwise specified, all steps of the present invention may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0070] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0071] If not specifically stated, in the present invention, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0072] The recombinant human collagen type III (molecular weight 55KD) and recombinant human collagen type IV (molecular weight 150-200KD) used in the following examples and comparative examples were purchased from Jiangsu Jiangshan Juyuan Biotechnology Co., Ltd.; glutamine endopeptidase (15.2U / μL enzyme solution) was purchased from Denmark Novozyme (China) Company; glutamine transaminase (English abbreviation: TGase, CAS: 80146-85-6, activity 200U / g) was purchased from Shanghai Yuanye Biotechnology Co., Ltd.; but not limited to the above manufacturers.
[0073] The polylysine used in the following examples and comparative examples has a Mw of 3800 to 4300, the Mw of polyglutamic acid is between 700000 and 1100000, the Mw of polyvaline is between 30000 and 70000, the Mw of polyleucine is between 40000 and 60000, the Mw of polyaspartic acid is between 6000 and 8000, the Mw of polythreonine is between 8000 and 10000, and the Mw of polycysteine is between 10000 and 20000.
[0074] The carbomer used in the following examples and comparative examples needs to be swollen in advance. Specifically, 10 g of carbomer is weighed and dissolved in 1 L of deionized water and allowed to stand for 6 hours.
[0075] The preparation method of the recombinant collagen composite gel in the following examples and comparative examples is to sequentially add recombinant collagen, polyamino acid, metal chloride, moisturizer, preservative, biocrosslinking agent and carbomer into water and dissolve them. It should be noted that stirring should be maintained during the addition of the raw materials, and the next raw material should be added after stirring evenly; when adding polyamino acid and biocrosslinking agent, stir and dissolve quickly, and pay attention to delay stirring of the beaker wall during stirring to avoid the generation of bubbles.
[0076] Example 1
[0077] The recombinant collagen composite gel of this example is composed of the following raw materials in percentage by mass: 0.15% recombinant type III human collagen, 4% polyglutamic acid, 0.1% transglutaminase, 2.5% sodium chloride, 0.5% carbomer 981, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the balance water. The obtained recombinant collagen composite gel sample is shown in the figure below: Figure 1 (a).
[0078] Example 2
[0079] The recombinant collagen composite gel of this example is composed of the following raw materials in percentage by mass: 0.15% recombinant type III human collagen, 4% polyglutamic acid, 0.1% transglutaminase, 2.0% sodium chloride, 0.5% carbomer 981, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the balance water. The obtained recombinant collagen composite gel sample is shown in the figure below: Figure 1 (b).
[0080] Example 3
[0081] The recombinant collagen composite gel of this example is composed of the following raw materials in percentage by mass: 0.2% recombinant type IV human collagen, 4% polyvaline, 0.1% transglutaminase, 2.0% sodium chloride, 0.5% carbomer U20, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the balance water. The obtained recombinant collagen composite gel sample is shown in the figure below: Figure 1 (c).
[0082] Example 4
[0083] The recombinant collagen composite gel of this example is composed of the following raw materials in percentage by mass: 0.15% recombinant type IV human collagen, 6% polyleucine, 0.1% transglutaminase, 2.5% sodium chloride, 0.5% carbomer 2020, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the balance water. The obtained recombinant collagen composite gel sample is shown in the figure below: Figure 1 (d).
[0084] Example 5
[0085] The recombinant collagen composite gel of this embodiment is composed of the following raw materials in percentage by mass: 0.5% recombinant human type III collagen, 6% polyaspartic acid, 0.1% transglutaminase, 2.5% potassium chloride, 0.5% carbomer 2020, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the remainder water.
[0086] Example 6
[0087] The recombinant collagen composite gel of this embodiment is composed of the following raw materials in percentage by mass: 0.4% recombinant type III human collagen, 6% polythreonine, 0.1% transglutaminase, 2.5% zinc chloride, 0.5% carbomer 2020, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the remainder water.
[0088] Example 7
[0089] The recombinant collagen composite gel of this embodiment is composed of the following raw materials in percentage by mass: 0.3% recombinant type III human collagen, 6% polycysteine, 0.1% transglutaminase, 2.5% zinc chloride, 0.5% carbomer 2020, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the remainder water.
[0090] Example 8
[0091] The recombinant collagen composite gel of this embodiment is composed of the following raw materials in percentage by mass: 0.3% recombinant human type III collagen, 0.15% recombinant human type IV collagen, 10% polyglutamic acid, 0.1% transglutaminase, 2.5% sodium chloride, 0.5% carbomer 2020, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the remainder water.
[0092] Example 9
[0093] The recombinant collagen composite gel of this embodiment is composed of the following raw materials in percentage by mass: 0.3% recombinant type III human collagen, 3% polyglutamic acid and 5% polylysine, 0.1% transglutaminase, 2.5% potassium chloride, 0.5% carbomer 2020, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the balance water.
[0094] Example 10
[0095] The recombinant collagen composite gel of this embodiment is composed of the following raw materials in percentage by mass: 0.4% recombinant human type III collagen, 0.1% recombinant human type IV collagen, 1% polyglutamic acid, 3% polylysine, 5% polyleucine, 0.1% transglutaminase, 2.5% sodium chloride, 0.5% carbomer 2020, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the remainder water.
[0096] Embodiment 11
[0097] The recombinant collagen composite gel of this embodiment is composed of the following raw materials in percentage by mass: 0.15% recombinant type III human collagen, 4% polyglutamic acid, 0.1% transglutaminase, 5% sodium chloride, 0.5% carbomer 981, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the balance water.
[0098] Example 12
[0099] The recombinant collagen composite gel of this embodiment is composed of the following raw materials in percentage by mass: 0.15% recombinant type III human collagen, 4% polyglutamic acid, 0.1% transglutaminase, 1% sodium chloride, 0.5% carbomer 981, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the balance water.
[0100] Example 13
[0101] The recombinant collagen composite gel of this embodiment is composed of the following raw materials in percentage by mass: 0.1% recombinant type IV human collagen, 3% polyvaline, 0.1% transglutaminase, 2.0% sodium chloride, 0.5% carbomer U20, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the balance water.
[0102] Embodiment 14
[0103] The recombinant collagen composite gel of this embodiment is composed of the following raw materials in percentage by mass: 0.2% recombinant type IV human collagen, 3% polyvaline, 0.1% transglutaminase, 2.0% sodium chloride, 0.5% carbomer U20, 3% glycerol, 0.1% methylparaben and the balance water.
[0104] Embodiment 15
[0105] The recombinant collagen composite gel of this embodiment is composed of the following raw materials in percentage by mass: 0.2% recombinant type IV human collagen, 3% polyaspartic acid, 0.1% glutamyl endopeptidase, 2.0% sodium chloride, 0.5% carbomer U20, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the balance water.
[0106] Example 16
[0107] The recombinant collagen composite gel of this example is composed of the following raw materials in percentage by mass: 0.2% recombinant type IV human collagen, 3% polylysine, 0.1% transglutaminase, 2.0% sodium chloride, 0.5% carbomer U20, 0.1% methylparaben and the balance water.
[0108] Embodiment 17
[0109] The recombinant collagen composite gel of this example is composed of the following raw materials in percentage by mass: 0.2% recombinant type IV human collagen, 3% polylysine, 0.1% transglutaminase, 2.0% sodium chloride, 0.5% carbomer U20, 3% glycerol and the balance water.
[0110] The present invention relates to a recombinant collagen composite gel, the main components of which include recombinant collagen, polyamino acids and biocrosslinking agents. The recombinant collagen uses recombinant human collagen, which has low antigenicity, good biocompatibility and high cell adhesion, and can promote the growth of skin cells and wound healing. The polyamino acid material itself has excellent biocompatibility and biodegradability. In addition, the polyamino acids in the gel of the present invention also have the advantages of providing viscosity and water retention, as well as enhancing the mechanical stability of the gel, which is crucial for promoting wound healing. In the preparation process of the gel, glutamine transaminase plays a key role. It can efficiently catalyze the formation of amide bonds between the amide groups of glutamine residues within or between molecules of recombinant collagen and the amino groups of lysine residues, thereby achieving crosslinking. The principle is detailed in Figure 2 Glutamyl endopeptidase is a chymosin-like enzyme with a serine residue as the active center. The enzyme specifically cleaves the peptide bond formed between the C-terminus of the protein polypeptide chain and the α-carboxyl group of the amino acid residue, thereby releasing the hydrophobic core region, which plays a hydrophobic modification role and further promotes protein aggregation. The biocrosslinking agent of the present invention has excellent biocompatibility and biodegradability, is non-toxic, and can also improve various aspects of the gel performance.
[0111] Comparative Example 1
[0112] The recombinant collagen composite gel of this comparative example is composed of the following raw materials in percentage by mass: 0.15% recombinant type III human collagen, 4% polyglutamic acid, 0.1% transglutaminase, 0.5% carbomer 981, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the balance water.
[0113] Comparative Example 2
[0114] The recombinant collagen composite gel of this comparative example is composed of the following raw materials in percentage by mass: 0.15% recombinant type III human collagen, 4% polyglutamic acid, 0.1% transglutaminase, 0.7% sodium chloride, 0.5% carbomer 981, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the balance water.
[0115] Comparative Example 3
[0116] The recombinant collagen composite gel of this comparative example is composed of the following raw materials in percentage by mass: 0.2% recombinant type IV human collagen, 0.1% transglutaminase, 2.0% sodium chloride, 0.5% carbomer 981, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the balance water.
[0117] Comparative Example 4
[0118] The recombinant collagen composite gel of this comparative example is composed of the following raw materials in percentage by mass: 0.15% recombinant type IV human collagen, 13% polyglutamic acid, 0.1% transglutaminase, 2.5% sodium chloride, 0.5% carbomer 981, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the balance water.
[0119] Comparative Example 5
[0120] The recombinant collagen composite gel of this comparative example is composed of the following raw materials in percentage by mass: 0.05% recombinant type III human collagen, 6% polyaspartic acid, 0.1% transglutaminase, 2.5% potassium chloride, 0.5% carbomer 981, 3% glycerol, 0.1% methylparaben, 0.5% phenoxyethanol and the balance water.
[0121] Effect Example 1——Performance Parameters
[0122] The performance parameters of the above comparative examples and embodiments are shown in Table 1.
[0123] Viscosity test method: The shear viscosity characterization method in the pharmaceutical industry standard of the People's Republic of China YY / T 0308-2015 "Sodium Hyaluronate Gel for Medical Use" is to use a rheometer (Shanghai Baosheng RH-30) at a shear rate of 0.001s -1 -1000s -1 Perform peristaltic scanning.
[0124] Collagen content test method: Test according to the fourth method of protein content determination method of the "Pharmacopoeia of the People's Republic of China" (General Rules of Part Four 0731), 2,2'-biquinoline-4,4'-dicarboxylic acid method (BCA method).
[0125] Water retention rate test method: Place the gel sample (w0) in gauze and soak it in water at a constant temperature of 37°C. Weigh the wet weight of the gel every 24 hours. After constant weight (w), calculate the water retention rate by the formula (w-w0) / w0×100%. Friction coefficient test method: Test according to GB 10006-88 / ISO 8295-1986 using MXD-02 friction coefficient meter.
[0126]
[0127] Generally, the addition of moisturizers is believed to increase the water retention capacity of the gel. Although no moisturizer is added in Example 16, the support structure of the polyamino acid and the network structure formed by the recombinant collagen catalyzed by the biocrosslinker play a decisive role in the water retention of the gel. Therefore, even if the water retention rate of Example 16 is relatively low, the design of this structure has provided the gel with good water retention capacity. However, in the actual product application process, the addition of moisturizers can further enhance the feel of the product and make it more in line with the expectations and needs of consumers. No preservatives are added in Example 17, so the gel product needs to be sealed and stored after sterilization.
[0128] Since no porogen is added or the amount of porogen added in Comparative Examples 1 and 2 is too small, the water retention rate is lower than that of the normal examples, and the friction coefficient is higher and the lubricity is relatively poor.
[0129] In comparative example 3, no polyamino acid is added, which results in poor overall mechanical properties of the gel, which is intuitively manifested in low gel viscosity and water retention rate.
[0130] In comparative example 4, adding too much polyamino acid will result in excessive gel viscosity and an increase in friction coefficient.
[0131] If the content of recombinant collagen used in Comparative Example 5 is too low, the collagen content of the gel will be too low, affecting its repair ability.
[0132] The gel product of the present invention has a shear viscosity of 22-30 Pa·s (22-26 Pa·s in a preferred embodiment), a water retention rate of 82-92% (85-92% in a preferred embodiment), and a friction coefficient of 0.11-0.17 (0.11-0.14 in a preferred embodiment).
[0133] Effect Example 2 - Aperture Effect
[0134] Figure 3 The SEM images of the gels prepared in Examples 1 to 4 are shown in FIG. 1 , wherein the SEM image of the gel in Example 1 is Figure 3 (a), SEM image of the gel in Example 2 Figure 3 (b), the gel of Example 3 is Figure 3 (c), the gel of Example 4 is Figure 3 (d) According to Figure 3 From the SEM images of the gels in Examples 1 to 4 and the results in Table 1, we can draw the following conclusions: adding a certain concentration of metal chloride can make the gel form a porous structure (see Figure 3 ). This porous structure has a positive effect on improving the air permeability, water retention rate and friction coefficient of the gel, thereby improving its comfort performance and making the gel have better cell adhesion and proliferation ability (see Table 1). Metal chlorides were added in Examples 1 to 4, but not in Comparative Example 1. Large-pore porous gels were formed in Examples 1 to 4, and the pore size of the gel in Comparative Example 1 was much smaller than that in Examples 1 to 4 (see Figure 3~4 , the scale bars in the figure are all 100 μm). Further combined with the results in Table 1, the gel pore size of Comparative Example 1 is relatively small, resulting in poor water retention and air permeability, and a large friction coefficient, which in turn affects the comfort performance and repair ability of the gel.
[0135] Therefore, the right amount of metal chloride is crucial to optimizing the overall performance of the gel. However, the amount of metal chloride added in Comparative Example 2 is insufficient, and its effect on optimizing the gel performance is limited. This shows that the amount of metal chloride added needs to be controlled within an appropriate range to ensure that the gel can achieve optimal performance.
[0136] Effect Example 3 - Cytotoxicity Test
[0137] The cell viability was measured after L929 cells were cultured for 1, 3 and 5 days using the gel extracts prepared in the above examples and comparative examples. The specific results are shown in Table 2.
[0138] The specific test method is:
[0139] (1) Preparation of experimental culture medium: The gels prepared in each example and comparative example were sterilized by irradiation with cobalt 60 and then extracted with fresh RPMI1640 culture medium from Gibco, USA, with an extraction concentration of 1 g / mL. The particulate matter in the solution was removed by filtering with a filter with a pore size of 0.2 μm to prepare the experimental culture medium.
[0140] (2) Preparation of cell suspension: L929 cells were digested and centrifuged, and then counted by blood cell plate to prepare cell suspension.
[0141] (3) Cultivate cells: Dilute the cell suspension with culture medium (fresh RPMI1640 culture medium from Gibco, USA) to a cell density of 1×10 4 / mL, and then inoculated in a 96-well plate at a volume of 100 μL per well, and each embodiment and comparative example set up six parallel experiments. Among them, the blank group had no cells but only culture medium, and the control group added cells and culture medium. After the cells were cultured for 24 hours to make them completely adhere to the wall, the culture medium of the control group was replaced with the experimental culture medium, and placed in an incubator for static culture.
[0142] (4) Calculation of cell viability (CCK-8 method): After one day (24 hours), remove the experimental culture medium and add CCK-8 solution, place in an incubator and let stand for 2 hours, then measure the absorbance of the solution. The same method is used to treat and detect cells cultured in the experimental culture medium for three days (72 hours) and five days (120 hours) to obtain cell viability. Among them, CCK-8 is a stain that can indirectly detect the number of living cells and can be used to analyze cytotoxicity.
[0143]
[0144] Effect Example 4 - Wound Repair Animal Experiment
[0145] In the full-thickness skin defect repair study, New Zealand rabbits were used in the experiment after being isolated for one week. The experimental design is as follows:
[0146] (1) Ten square full-thickness skin wounds with a side length of 1 cm were cut from the back of each rabbit, with a distance of 2 cm between the wounds. The wounds were disinfected with iodine tincture.
[0147] (2) Experimental group: The gel prepared in Examples 1 to 4 was applied to the wounds of four rabbits respectively, and photos of the full-thickness skin defects on the first day were taken. The full-thickness skin wounds were then covered with polyurethane film and vaseline gauze in turn.
[0148] (3) Control group: Take photos of the rabbits’ full-thickness skin defects on the first day, which are only covered with polyurethane film and vaseline gauze in sequence.
[0149] (4) The rabbits were placed in cages, and the gel in the experimental group was replaced every three days to ensure the integrity of the dressing and the normal healing process of the wound; the polyurethane film and vaseline gauze in the control group were only replaced every three days.
[0150] (5) After cleaning the wound on the 3rd, 7th, and 15th days, take photos to record the repair of the full-thickness skin defect.
[0151] from Figure 5 ( Figure 5The length of the middle ruler corresponds to 5 mm). It can be seen that the wounds treated with Examples 1, 2, 3 and 4 did not show purulent tissue and produced new granulation tissue, because the gel isolated external bacteria and dust to prevent wound infection, provide nutrition, and promote wound healing. The wounds treated with Examples 3 and 4 healed better than the untreated wounds on the 7th and 15th days. The promotion effect of Examples 1 and 2 was better, but the difference was not significant.
[0152] Effect Example 5 - Efficacy of gel combined with LED irradiation in treating facial dermatitis
[0153] (1) Observation group and control group
[0154] The control group used KN-7000DLED spectrum therapy device for LED irradiation treatment (red light energy density was set to 40mW / cm², wavelength 630nm; yellow light energy density was set to 30mW / cm², wavelength 590nm). Patients were required to close their eyes and wear eye masks during treatment, and the distance between the light source and the face was kept at 10 to 15cm. Red light and yellow light were alternately irradiated on the face for 10 minutes each time, twice a week. Continue for 4 weeks. The observation group applied the dressing prepared in Example 1 to the irradiated area for 30 minutes immediately after the irradiation treatment of the control group.
[0155] (2) Evaluation indicators and judgment criteria
[0156] Skin lesion symptoms (telangiectasia, erythema, papules, dryness, desquamation, itching, burning, tightness) were scored according to severity (none for 0, mild for 1, moderate for 2, severe for 3), the total score of skin lesion severity before and after treatment was calculated, and the clinical efficacy of the two groups of patients was evaluated. Among them, the efficacy index = (pre-treatment score-post-treatment score) / pre-treatment score × 100%, > 90% is cured, 60%-90% is markedly effective, 20%-59% is improved, and < 20% is ineffective.
[0157] Cure rate = number of cured people / total number of people (n) × 100%, markedly effective rate = number of markedly effective people / total number of people (n) × 100%, effective rate = cure rate + markedly effective rate, and the effective rate is used to evaluate the efficacy.
[0158] (3) Efficacy of the two groups of patients
[0159] Clinical research results: For the lesion severity score, there was no statistically significant difference in the lesion symptom severity score between the two groups before treatment (P>0.05); after treatment, the lesion severity scores of the two groups were lower than before treatment (P<0.05), and the lesion severity scores of the observation group after treatment were significantly lower than those of the control group (P<0.05), see Table 3. For the direct clinical efficacy, the clinical effective rate of the observation group was higher than that of the control group (P<0.05), the efficacy of the observation group reached 90.39%, and the efficacy of the control group was only 71.43%, see Table 4.
[0160]
[0161]
[0162] In statistics, the t value is a statistic used to compare the difference between the sample mean and the population mean; the P value is a probability value used to determine the results of a hypothesis test; 2 The value in the chi-square test is a mathematical statistic calculated based on the normal distribution; n refers to the sample size or degrees of freedom, where n refers to the number of patients.
[0163] Recombinant collagen composite polyamino acid gel and dressing products can be sterilized by irradiation before packaging. After irradiation sterilization, the gel and dressing still maintain viscosity and will not have the problem of product viscosity reduction. As a high-molecular material with high biosafety, polyamino acid can be added to the system to prevent the problem of system viscosity reduction after radiation sterilization.
[0164] The medical gel containing recombinant humanized collagen of the present invention has a mild component. It utilizes recombinant humanized collagen and polyamino acids in combination. In addition to better exerting the moisturizing, penetrating and repairing effects of recombinant humanized collagen, it is suitable for the care of non-chronic wounds, provides a microenvironment for wound healing, inhibits and alleviates skin inflammatory reactions, promotes wound healing, reduces the risks of post-inflammatory pigmentation and scar formation, improves the skin, and delays skin aging.
[0165] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods. The specific embodiments described above further describe the purpose, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A recombinant collagen composite gel, characterized in that: The preparation method comprises the following raw materials: 0.1-0.5wt% recombinant collagen, 3-10wt% polyamino acid, 0.1-0.4wt% biological cross-linking agent, 0.3-1wt% carbomer and 1-5wt% metal chloride; The recombinant collagen is at least one of recombinant type III human collagen and recombinant type IV human collagen; The biological cross-linking agent is transglutaminase or glutamyl endopeptidase; The metal chloride is at least one of sodium chloride, potassium chloride and zinc chloride; The polyamino acid is at least one of polylysine, polyglutamic acid, polyvaline, polyleucine, polyaspartic acid, polythreonine and polycysteine.
2. The recombinant collagen composite gel according to claim 1, characterized in that: The method comprises 0.15-0.45 wt% of recombinant collagen, 4-8 wt% of polyamino acid, 0.1-0.2 wt% of biological cross-linking agent and 2-3 wt% of metal chloride.
3. The recombinant collagen composite gel according to claim 1, characterized in that: The recombinant collagen satisfies at least one of the following conditions (1)-(2): (1) The molecular weight of the recombinant human type III collagen is 35-60KD; (2) The molecular weight of the recombinant human type IV collagen is 150~200KD.
4. The recombinant collagen composite gel according to claim 1, characterized in that: The molecular weight of the polyamino acid is 3800-1100000.
5. The recombinant collagen composite gel according to claim 1, characterized in that: The polyamino acid satisfies at least one of the following conditions (1) to (7): (1) The molecular weight of the polylysine is 3800-4300; (2) The molecular weight of the polyglutamic acid is 700,000 to 1,100,000; (3) The molecular weight of the polyvaline is 30,000 to 70,000; (4) The molecular weight of the polyleucine is 40,000 to 60,000; (5) The molecular weight of the polyaspartic acid is 6000-8000; (6) The molecular weight of the polythreonine is 8000-10000; (7) The molecular weight of the polycysteine is 10,000 to 20,000.
6. The recombinant collagen composite gel according to claim 1, characterized in that: The carbomer is at least one of carbomer 941, carbomer 971, carbomer 981, carbomer U20 and carbomer 2020.
7. The recombinant collagen composite gel according to claim 1, characterized in that: The raw materials for its preparation also contain moisturizers and preservatives.
8. The recombinant collagen composite gel according to claim 7, characterized in that: It satisfies at least one of the following conditions (1)-(2): (1) The moisturizing agent is glycerin, propylene glycol or sodium hyaluronate; (2) The preservative is at least one of methylparaben and phenoxyethanol.
9. The recombinant collagen composite gel according to claim 7, characterized in that: It is composed of the following raw materials: Recombinant collagen 0.1-0.5wt%, polyamino acid 3-10wt%, carbomer 0.3-1wt%, metal chloride 1-5wt%, biocrosslinking agent 0.1-0.4wt%, preservative 0.1-0.9wt%, humectant 1-6wt% and balance water.
10. The recombinant collagen composite gel according to any one of claims 1 to 9, characterized in that: The preparation method comprises the steps of mixing the preparation raw materials.
11. A recombinant collagen composite dressing, characterized in that: It comprises the recombinant collagen composite gel as described in any one of claims 1 to 10.
12. Use of the recombinant collagen composite gel as claimed in any one of claims 1 to 9, or the recombinant collagen composite dressing as claimed in claim 11, in the preparation of a product for treating non-chronic wounds and / or skin inflammation.