An indirect bonding method of erbium glass and cobalt spinel
By designing the film system structure and ion beam sputtering technology on the bonding surface of erbium glass and cobalt spinel, the intensity and light transmittance are improved, and the interface damage and insufficient firmness of the light glue are solved. It is suitable for high-temperature lasers stable bonding and integration.
Patent Information
- Application Number
- CN202410264990.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-08
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-03-08
AI Technical Summary
The existing bonding methods of erbium glass and cobalt spinel have problems such as interface damage, low damage threshold, insufficient fiberglue firmness and difficulty in bonding large devices, especially due to lattice mismatch and instability at the bonding site. This leads to easy damage to the material, affecting the stability and light transmittance of the laser.
Indirect bonding method is adopted, including pretreatment of the surface of erbium glass and cobalt spinel, plating SiO2 film and plating Al2O3 film through ion beam sputtering technology, and after surface activation, photoglue and heating and pressurization bonding are carried out in the vacuum chamber. Ensure bonding surface strength and light transmittance.
It improves the interface intensity and light transmittance of the bonded crystal, lowers the damage threshold, enhances the bonding stability and processing convenience of large devices, and is suitable for laser applications under high temperature conditions.
Smart Images

Figure CN118344171B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of bonding methods for solid laser crystals, in particular to a bonding method for erbium glass and cobalt spinel. Background Art
[0002] 1.5μm-1.8μm is an eye-safe band. The 1.5μm band laser is in the atmospheric transmission window, has strong penetration ability to smoke, etc., and has low transmittance to the human eye. It has a very high safety factor and can be used as an ideal eye-safe laser band for laser ranging. The 1.5μm band micro-range laser currently developed is highly compact, small in size, highly temperature-adaptable, and low in cost, and is widely used in civil markets such as engineering exploration and geological research.
[0003] Since erbium ions can obtain lasers with a wavelength of about 1.5 μm through energy level transitions, laser output of this wavelength has been achieved in a variety of glass and crystal media. For LD-pumped erbium glass lasers, cobalt spinel is usually used as a saturable absorber for passive q-switching and for outputting high-power pulsed lasers. For example, a 1.5-micron wavelength hot bond and composite laser crystal preparation mentioned in patent publication number CN 108823639 A is usually combined between erbium glass and cobalt spinel through hot bonding technology to reduce the volume of the laser and increase the heat dissipation capacity of the crystal. However, after the cobalt spinel and erbium glass are bonded, the resonant cavity is very short, resulting in a very narrow pulse width and a very high peak power, which easily reaches the damage threshold, causing damage to the material and film and reducing the stability of the laser. In addition, there is a lattice mismatch problem between cobalt spinel and erbium glass, and the joint is not strong enough.
[0004] At present, the indirect bonding methods are mainly divided into adhesive bonding technology, low-temperature eutectic bonding technology, and low-temperature vacuum bonding technology. Among them, adhesive bonding uses polymer as the intermediate medium, and the bonding strength of the polymer intermediate layer is general and easy to age, which is not conducive to practical application; while the low-temperature eutectic technology uses homogeneous alloys to bond at the interface, but metals generally have poor light transmittance and cannot guarantee the transmittance of light at the interface; low-temperature vacuum bonding technology is also called ion-assisted bonding technology. Before wafer bonding, the surface is activated with plasma. Surface activation mainly increases dangling bonds through mechanical impact and sputtering of ions on the wafer surface, empowering the wafer surface. The activated surface has a strong adsorption capacity. At a lower temperature, the wafer bonding interface can have a higher bonding strength. Therefore, low-temperature vacuum bonding technology is a better choice, but under normal circumstances, the bonding layer material of low-temperature vacuum bonding will seriously damage the transmission of light.
[0005] Therefore, there is an urgent need for an indirect bonding method of erbium glass and cobalt spinel that can solve the above problems. Summary of the invention
[0006] The present invention provides an indirect bonding method of erbium glass and cobalt spinel, with the aim of solving some problems existing in the above-mentioned high-temperature bonding crystals of erbium glass and cobalt spinel for 1.5μm solid-state lasers: damage exists at the interface, which reduces the damage threshold and makes it easy for the interface to spark; the firmness of the optical glue is insufficient and the interface is easy to detach; it is difficult to bond large devices, mainly because the surface flatness of large devices fluctuates greatly and the firmness of the joints is insufficient.
[0007] The specific scheme of the present invention is as follows: an indirect bonding method of erbium glass and cobalt spinel, comprising the following steps:
[0008] S1 selects appropriate erbium glass and cobalt spinel as bonding crystals;
[0009] S2 performs surface treatment on the pre-bonded surfaces of erbium glass and cobalt spinel respectively;
[0010] S3 coats the pre-bonded surface of the cobalt spinel treated by S2 with SiO2 film;
[0011] S4 puts the surface-treated erbium glass in S2 and the film-treated cobalt spinel in S3 into a vacuum chamber and plates an Al2O3 film of the same thickness by ion beam sputtering technology to activate the bonding surfaces of the two materials;
[0012] S5 performs photoresist coating on the coated surfaces of the two materials in a vacuum chamber for the crystals that have been surface activated by S4;
[0013] S6: bonding the cobalt spinel and erbium glass after S4 by heating and pressurizing in a vacuum chamber to obtain a bonded crystal;
[0014] The bonded crystals obtained by the S6 treatment were subjected to a bonding strength tensile test and a cutting test, and the bonded crystals obtained by the S6 treatment were subjected to an interface loss test.
[0015] Preferably, the erbium glass is phosphate glass or silicate glass, both of which have stress values less than 20 and are defect-free.
[0016] Preferably, after the surface treatment in step S2, the bonding surface of the obtained erbium glass and cobalt spinel reaches a surface roughness Ra of 0.5-1.5 nm, a surface profile better than λ / 10, and a smoothness S / D of 10-5.
[0017] Preferably, in step S3, the thickness of the SiO2 film plated on the pre-bonding surface of the cobalt spinel is 100-500 nm.
[0018] Preferably, in step S4, the erbium glass and the cobalt spinel coated with SiO2 film are coated with Al2O3 films of the same thickness by ion beam sputtering at a pressure below 5*10^-4Pa using an Al target and an oxygen atmosphere.
[0019] Preferably, in step 6), the temperature is raised and the pressure is applied in a vacuum chamber for bonding. Under a pressure of 35-80 kg, the temperature is slowly raised to 250-350° C. at a rate of 10-25° C. / h, maintained at a constant temperature for 48-96 hours, and then cooled to room temperature at the same cooling rate.
[0020] Preferably, the bonding strength test and cutting test of the bonded crystal are carried out, and the tensile strength of the interface is tested by a tensile tester; the destructive inner circle cutting experiment is carried out to determine whether the interface is damaged after cutting a 1*1*L square strip.
[0021] Preferably, the bonded crystal is subjected to an interface loss test, a PCI weak absorption tester is used to test the interface absorption using a 1064nm wavelength light source, and a 1064nm laser damage threshold test system is used to test the interface damage threshold.
[0022] The present invention provides an indirect bonding method of erbium glass and cobalt spinel, which can perfectly solve the problems of damage at the interface when erbium glass and cobalt spinel are bonded at high temperature, reduce the damage threshold, and easily spark the interface; the optical glue is not strong enough, and the interface is easy to detach; it is difficult to bond large devices, mainly including large fluctuations in surface flatness of large devices and insufficient firmness of the joints. The present invention designs a film system structure at the bonding surface: erbium glass + Al2O3 + Al2O3 + SiO2 + cobalt spinel, on the one hand, it ensures that light can be transmitted at the interface, and on the other hand, through the method of ion beam sputtering, the bonding surface is surface activated to enhance the bonding strength at the bonding surface, and the crystal bonded by this method can be more convenient to process and integrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the following briefly introduces the drawings required to be used in the embodiment of the present invention.
[0024] Figure 1 , is a flow chart of the indirect bonding method of erbium glass and cobalt spinel;
[0025] Figure 2 , is a front view of SiO2 film plated on the surface of cobalt spinel after step 3);
[0026] Figure 3 , is a front view of the two materials after the ion beam sputtering treatment on the bonding surface of the erbium glass and the cobalt spinel in step 4);
[0027] Figure 4, is a schematic diagram of the final bonded crystal;
[0028] Reference numerals: (1) erbium glass, (2) cobalt spinel, (3) SiO2 thin film, (4, 4') Al2O3 layer; DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0030] In view of the existing technical problems, the present invention provides an indirect bonding method of erbium glass and cobalt spinel. First, after the surfaces of the two materials are treated, a layer of SiO2 film is plated on the surface of the cobalt spinel; after cleaning, the cobalt spinel and the erbium glass are simultaneously sputtered with Al203 of the same thickness on the bonding surface by an ion beam sputtering method to activate the bonding surface; after the surface activation, the coated surfaces of the two materials are photobonded in a vacuum chamber, and then pressure is applied to the two materials after photobonding by a hydraulic device in the vacuum chamber, and the temperature is increased at a certain rate, so as to obtain a bonded crystal.
[0031] like Figure 1 Shown is a flow chart of the indirect bonding method of erbium glass and cobalt spinel.
[0032] Example 1
[0033] An indirect bonding method of erbium glass and cobalt spinel comprises the following steps:
[0034] 1) Material selection. In this embodiment, the erbium glass and cobalt spinel raw materials with uniform internal stress and stress value less than 20 are first selected by a stress analyzer, and raw materials without defects such as envelope, scattering and grain boundary are selected by an optical material inspection method. The erbium glass is a phosphate matrix glass co-doped with erbium and ytterbium. Both materials are 20*20*Lmm thick;
[0035] 2) Surface treatment of the two materials, including polishing and cleaning. Through the ultra-smooth surface polishing process, the polishing finish of bait glass and spinel is S / D: 10-5, the roughness is 0.8nm after testing with Zygo white light interferometer, the surface shape is better than 1 / 10λ and the parallelism is better than 5″ after testing with Zygo plane interferometer. The final products are 20*20*3mm respectively, and then the two materials are cleaned; the above parameters are to ensure the yield of optical glue and bonding in the later stage;
[0036] 3) Evaporate SiO2 film on the bonding surface of cobalt spinel. First, put the polished and cleaned CoSpinel into the coating machine, adjust the coating machine state and vacuum evaporate 300nm SiO2 film to obtain a crystal such as Figure 2 As shown;
[0037] 4) Place the cobalt spinel coated with SiO2 film in 3) and the erbium-ytterbium co-doped phosphate glass after polishing and cleaning in 2) into a vacuum coating machine and evacuate the vacuum to a vacuum degree of 1.0*10 -5 Pa, using aluminum target and oxygen atmosphere, ion beam sputtering technology was used to coat Al2O3 film on the bonding surface of cobalt spinel and erbium glass. The film thickness was 60-85nm and the bonding surface was activated. After treatment, the crystal was Figure 3 shown.
[0038] 5) photo-bonding the coated surfaces of the cobalt spinel and erbium glass after coating and surface activation in 4) in a vacuum chamber;
[0039] 6) Apply 50 kg pressure to the product after photoresist through the hydraulic device in the vacuum chamber, slowly increase the temperature to 300°C at a rate of 15°C / h, keep the temperature constant for 72 hours, slowly cool down to room temperature at a rate of 15°C / h, and then take out the bonded crystal. The resulting bonded crystal is as follows: Figure 4 As shown;
[0040] 7) The bonded crystal obtained in 6) is tested for interface tensile strength by a tensile tester, and the interface strength per unit area is greater than 30Kg / cm 2 ; A destructive inner circle cutting experiment was performed on the bonded crystal obtained in 6), and after cutting 1*1*L square strips, there was no damage to the interface;
[0041] 8) The bonded crystal obtained in 6) was tested using a PCI weak absorption tester with a 1064nm wavelength light source, and the interface weak absorption was measured to be less than 200ppm; the interface damage threshold was tested using a 1064nm laser damage threshold test system and was greater than 25J / cm2@1064nm@10ns,10Hz.
[0042] Through the above steps, a bonded crystal of erbium-ytterbium co-doped phosphate glass and cobalt spinel with good light transmittance at the interface, weak absorption, high damage threshold and strong bonding strength is obtained.
[0043] Example 2
[0044] An indirect bonding method of erbium glass and cobalt spinel comprises the following steps:
[0045] S1 Material selection. In this embodiment, the erbium glass and cobalt spinel raw materials with uniform internal stress and stress value less than 20 are first selected by a stress analyzer, and raw materials without defects such as envelope, scattering and grain boundary are selected by an optical material inspection method. The erbium glass is a silicate matrix glass co-doped with erbium and ytterbium. Both materials are 20*20*Lmm thick;
[0046] S2 performs surface treatment on the two materials, and the surface treatment includes two steps of polishing and cleaning. Through the ultra-smooth surface polishing process, the polishing finish S / D of erbium glass and spinel is achieved: 10-5. After testing with Zygo white light interferometer, the roughness of erbium glass is 0.8nm and the roughness of cobalt spinel is 0.6nm. The surface shape is better than 1 / 10λ and the parallelism is better than 5″ measured by Zygo plane interferometer. The final products are 20*20*3mm respectively, and then the two materials are cleaned; the above parameters are to ensure the yield of optical glue and bonding in the later stage;
[0047] S3 evaporates SiO2 film on the bonding surface of cobalt spinel, first puts the polished and cleaned CoSpinel into the coating machine, adjusts the coating machine state and then vacuum evaporates 300nm SiO2 film;
[0048] S4 puts the cobalt spinel coated with SiO2 film in S3 and the erbium-ytterbium co-doped phosphate glass after polishing and cleaning in 2) into a vacuum coating machine, and evacuates the vacuum to a vacuum degree of 1.0*10 -5 Pa, using aluminum target and oxygen atmosphere, ion beam sputtering technology is used to coat Al2O3 film on the bonding surface of cobalt spinel and erbium glass. The film thickness is 60-85nm and the bonding surface is surface activated.
[0049] S5 performs photo-bonding on the coated surface of the cobalt spinel and erbium glass after coating and surface activation in S4 in a vacuum chamber;
[0050] S6 applies 50Kg of pressure to the product after photoresist bonding through the hydraulic device in the vacuum chamber, slowly raises the temperature to 350℃ at a rate of 15℃ / h, keeps the temperature constant for 48h, and slowly cools down to room temperature at a rate of 20℃ / h before taking out the bonded crystal;
[0051] The bonded crystal obtained in S6 was tested for interface tensile strength using a tensile tester, and the interface strength per unit area was greater than 35Kg / cm 2 ; A destructive inner circle cutting experiment was carried out on the bonded crystal obtained in S6. After cutting 1*1*L square strips, there was no damage to the interface;
[0052] The bonded crystal obtained in S6 was tested using a PCI weak absorption tester with a 1064nm wavelength light source, and the interface weak absorption was measured to be less than 220ppm; the interface damage threshold was tested using a 1064nm laser damage threshold test system and was found to be greater than 25J / cm2@1064nm@10ns,10Hz.
[0053] Through the above steps, a bonded crystal of erbium-ytterbium co-doped silicate matrix glass and cobalt spinel with good light transmittance at the interface, weak absorption, high damage threshold and strong bonding strength is obtained.
[0054] Comparative Example 1
[0055] A high temperature bonding method of erbium glass and cobalt spinel, the process is as follows:
[0056] 1) Selecting and preparing erbium glass and cobalt spinel with a surface size of 10×10 mm as gain medium and Q crystal, wherein the erbium glass is Er and Yb co-doped phosphate glass;
[0057] 2) Polish and clean the cobalt spinel and erbium glass respectively, so that the surface roughness of both reaches Ra<0.5nm and the surface shape is better than λ / 10;
[0058] 3) After polishing and cleaning in 2), wipe the crystal and glue it in a clean room to form a photocolloid. The two materials are closely attached. The surface of the photocolloid and photocolloid is examined under an optical microscope with a magnification of 100 times. The diameter of the bubble or impurity particle defect must be less than 1μm.
[0059] 4) After confirming that there are no defects between the crystals after the photoresist, a high-temperature bonding sintering process is performed: the photoresist is placed vertically on the alumina ceramic plate without tilting, and then the ceramic plate is placed in a constant temperature sintering furnace. The constant temperature sintering furnace adopts a vacuum atmosphere. The constant temperature sintering furnace slowly heats up from room temperature to 200°C at a rate of 40°C / h and keeps the temperature constant for 5h; then slowly heats up to 520°C at a rate of 20°C / h and keeps the temperature constant for 30h; the constant temperature furnace is heated to a vacuum degree of <1×10 -3 Pa when the temperature is increased;
[0060] 5) slowly cooling the constant temperature sintering furnace from the highest temperature to room temperature at a cooling rate of 20° C. / h to obtain a high temperature bonded crystal;
[0061] 6) Take out the bonded crystal obtained in 5) and perform a bonding strength tensile test. Use a tensile tester to perform a tensile test. Make a suitable fixture to fix the two end faces of the crystal. Perform an axial tensile test and a transverse shear stress tensile test. The axial tensile test result is 20Kg / cm 2 , the transverse tensile test result is 15kg / cm 2 .
[0062] 7) After taking out the bonded crystal obtained in 5), a weak absorption tester is used to perform interface scanning. The experimental results show that the weak absorption at the cross section is 300 ppm, which meets the laser cross section loss condition.
[0063] The same materials are used for bonding in Comparative Example 1 and Example 1. Example 1 uses indirect bonding technology, while Comparative Example 1 uses high-temperature direct bonding technology to bond cobalt spinel and erbium-ytterbium co-doped phosphate glass. The parameters of the three solutions are shown in Table 1.
[0064] Table 1. Test results.
[0065]
[0066] In comparison, the temperature in Comparative Example 1 is higher. According to the literature, the softening temperature of phosphate glass is around 450-500 degrees Celsius, so the glass may be damaged, thereby reducing the bonding strength and weakening the damage threshold at the bonding surface. The test data provided in Table 1 also proves this point, that is, the indirect bonding technology of erbium glass and cobalt spinel is more effective and can provide higher bonding strength, higher damage threshold and lower interface loss.
[0067] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principles of the present invention shall be equivalent replacement modes and shall be included in the protection scope of the present invention.
Claims
1. An indirect bonding method of erbium glass and cobalt spinel, characterized in that: The method comprises the following steps: S1 selects appropriate erbium glass and cobalt spinel as bonding crystals; S2 performs surface treatment on the pre-bonded surfaces of erbium glass and cobalt spinel respectively; S3 coats the pre-bonded surface of the cobalt spinel treated by S2 with a SiO2 film, and cleans the surface; S4 puts the surface-treated erbium glass in S2 and the film-treated cobalt spinel in S3 into a vacuum chamber and plates Al2O3 thin film by ion beam sputtering technology to activate the bonding surfaces of the two materials; S5 performs photoresist coating on the coated surfaces of the two materials in a vacuum chamber for the crystal whose surface has been activated in S4; S6 bonds the cobalt spinel and erbium glass after optical bonding in S5 by increasing temperature and applying pressure in a vacuum chamber to obtain a bonded crystal.
2. The indirect bonding method of erbium glass and cobalt spinel according to claim 1, characterized in that: The erbium glass and cobalt spinel in step S1 should be made of raw materials with a stress value less than 20 and no defects.
3. The indirect bonding method of erbium glass and cobalt spinel according to claim 1, characterized in that: The erbium glass in step S1 may be erbium-ytterbium co-doped phosphate-based glass or silicate-based glass.
4. The indirect bonding method of erbium glass and cobalt spinel according to claim 1 is characterized in that: The surface treatment in step S2 is polishing and cleaning, so that the bonding surface of erbium glass and cobalt spinel reaches a surface roughness Ra of 0.5-1.5nm, a surface shape better than λ / 10, and a smoothness S / D of 10-5.
5. The indirect bonding method of erbium glass and cobalt spinel according to claim 1, characterized in that: In the step S3, the thickness of the SiO2 film coated on the pre-bonded surface of the cobalt spinel is 100-500nm.
6. The indirect bonding method of erbium glass and cobalt spinel according to claim 1, characterized in that: The step S4 is to plate the Al2O3 film by ion beam sputtering technology, using an Al target material and an oxygen atmosphere with a vacuum degree less than 5*10^-4Pa.
7. The indirect bonding method of erbium glass and cobalt spinel according to claim 1, characterized in that: The step S6 of heating and pressurizing the vacuum chamber for bonding is to slowly heat the temperature to 250-350° C. at a rate of 10-25° C. / h under a pressure of 35-80 kg, keep the temperature constant for 48-96 hours, and then cool down to room temperature at the same cooling rate.
8. The indirect bonding method of erbium glass and cobalt spinel according to claim 1, characterized in that: The bonded crystal obtained in step S6 needs to undergo a bonding strength tensile test and a cutting test.