Halogen-free flame-retardant modified plastic masterbatch and preparation method thereof

By introducing poly(biphenylmaleimide-DOPO-piperazine) flame retardant into the polyolefin resin and carrying out cross-linking reaction, the problems of insufficient high temperature resistance and flame retardant properties of polyolefin plastics are solved, and the problem of insufficient flame retardant properties of polyolefin plastics is achieved. Higher thermal decomposition temperature and flame retardant performance improvement.

CN118344670BActive Publication Date: 2024-11-05DONGGUAN G&K NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410456279.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-16
Publication Date
2024-11-05
Estimated Expiration
2044-04-16

AI Technical Summary

Technical Problem

The application of polyolefin plastics in fire-resistant and flame-resistant materials is due to their poor high temperature resistance and flame-retardant properties, and existing flame retardants have a negative impact on the mechanical properties and thermal decomposition temperature of the material.

Method used

Using poly(biphenylmaleimide-DOPO-piperazine) flame retardant, prepared by melt polymerization and acylation reaction, added to the polyolefin resin to form a crosslinked structure to improve the thermal decomposition temperature and flame retardant properties. , and grafting reaction occurs with polyolefins such as polypropylene through diisopropyl peroxide or ditert-butyl peroxide initiator.

Benefits of technology

It significantly improves the initial decomposition temperature and tensile strength of polyolefin materials, while significantly improving its ultimate oxygen index and flame retardancy, ensuring better high temperature resistance and flame retardancy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004794325120000041
    Figure BDA0004794325120000041
  • Figure BDA0004794325120000042
    Figure BDA0004794325120000042
  • Figure BDA0004794325120000071
    Figure BDA0004794325120000071
Patent Text Reader

Abstract

The present invention relates to the technical field of halogen-free flame-retardant plastic masterbatch, and discloses a halogen-free flame-retardant modified plastic masterbatch and a preparation method, including 84-96 parts by weight of polyolefin resin, 3-15 parts by weight of poly(biphenyl maleimide-DOPO-piperazine) flame retardant, 0.2-0.8 parts by weight of initiator, 0.2-0.5 parts by weight of antioxidant, the alkenyl maleimide group in the flame retardant of the present invention can be grafted and cross-linked with polyolefins such as polypropylene and polyethylene, so that the polyaromatic amide polymer containing maleimide rings and biphenyl structures with high thermal decomposition properties is cross-linked and grafted into the polypropylene molecular chain, so that the cross-linked polyolefins such as polypropylene have better high temperature resistance, and the tensile strength is significantly improved. At the same time, the limiting oxygen index and flame retardancy of the polyolefin are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of halogen-free flame-retardant plastic masterbatch, and in particular to a halogen-free flame-retardant modified plastic masterbatch and a preparation method thereof. Background Art

[0002] Polyolefin plastics mainly include polypropylene, polyethylene, polystyrene, polyvinyl chloride, etc. They have good processing properties and mechanical properties and are widely used in various fields of national economy and daily life. However, these polyolefin plastics have poor high temperature resistance and no flame retardant properties. This limits the application of polyolefin plastics in fireproof and flame retardant materials. At present, flame retardants are mainly used to modify polyolefin plastics. Therefore, the development of halogen-free and environmentally friendly flame retardants has become a research trend in recent years.

[0003] Halogen-free flame retardants mainly include nitrogen, phosphorus, silicon, etc.; expansion flame retardant is a new type of flame retardant that integrates carbon source, acid source and gas source, and has important applications in polyolefin plastics. Chinese patent CN112029157B discloses an anti-melting drop composite expansion flame retardant and its preparation method and application. Chitosan unsaturated carboxylic acid ester coats ammonium polyphosphate, and a cross-linked chitosan unsaturated carboxylic acid ester composite layer rich in carbon, phosphorus or sulfur is formed on the surface of ammonium polyphosphate to obtain a "three-in-one" composite expansion flame retardant, which has a good flame retardant for polyolefin materials. However, when flame retardants are added to materials such as polyolefins, due to poor compatibility, they will affect the mechanical properties of the materials. In addition, the thermal decomposition temperature of flame retardants such as nitrogen and phosphorus is usually low, and the addition will affect the thermal decomposition temperature and heat resistance of the material. Summary of the invention

[0004] The invention solves the problem that polypropylene German polyolefin plastic masterbatch has poor flame retardancy, high temperature resistance and other properties.

[0005] The technical solution of the present invention is a halogen-free flame retardant modified plastic masterbatch, comprising the following components: 84-96 parts by weight of polyolefin resin, 3-15 parts by weight of poly(biphenyl maleimide-DOPO-piperazine) flame retardant, 0.2-0.8 parts by weight of initiator, and 0.2-0.5 parts by weight of antioxidant.

[0006] The preparation method of the poly(biphenyl maleimide-DOPO-piperazine) flame retardant is as follows: nitrogen is introduced into a reaction kettle, 4,4'-(piperazine-1,4-diyl) diphenylamine, DOPO-maleic acid, and 3,3'-di(maleimide)-[1,1'-biphenyl]-4,4'-dicarboxylic acid are added, melt polymerization is carried out, cooling is performed after the reaction, washing is performed with ethanol, and drying is performed to obtain the poly(biphenyl maleimide-DOPO-piperazine) flame retardant.

[0007] Furthermore, the polyolefin resin includes at least one of polypropylene, polyethylene, polyvinyl chloride, and polystyrene.

[0008] Furthermore, the preparation method of the halogen-free flame retardant modified plastic masterbatch is as follows: polyolefin resin, poly(biphenyl maleimide-DOPO-piperazine) flame retardant, initiator, and antioxidant are added to a twin-screw extrusion rheometer, the screw speed is 60-150r / mn, extrusion, granulation, and halogen-free flame retardant modified plastic masterbatch.

[0009] Furthermore, the initiator is at least one of dicumyl peroxide and di-tert-butyl peroxide.

[0010] Furthermore, the ratio of 4,4'-(piperazine-1,4-diyl)diphenylamine, DOPO-maleic acid, and 3,3'-di(maleimide)-[1,1'-biphenyl]-4,4'-dicarboxylic acid is 1 mol:(0.6-0.85) mol:(0.15-0.4) mol.

[0011] Furthermore, the melt polymerization is controlled at a temperature of 260-270° C. and a time of 1-2 h.

[0012] Furthermore, the preparation method of N-isophthalic acid maleimide is: add N,N-dimethylformamide, 3,3'-diamino-[1,1'-biphenyl]-4,4'-dicarboxylic acid and maleic anhydride into a reaction container, carry out acylation reaction at 20-35°C for 12-18h, concentrate under reduced pressure, wash the intermediate with acetone, add acetic anhydride after drying, and then add sodium acetate, carry out cyclization reaction at 60-70°C for 4-8h, concentrate under reduced pressure, wash the product with water and acetone in turn, and dry to obtain N-isophthalic acid maleimide.

[0013] Furthermore, the ratio of 3,3'-diamino-[1,1'-biphenyl]-4,4'-dicarboxylic acid to maleic anhydride is 1 mol:(2.2-2.4) mol.

[0014] Technical effect: The present invention utilizes 3,3'-diamino-[1,1'-biphenyl]-4,4'-dicarboxylic acid and maleic anhydride to carry out acylation reaction and cyclization reaction to prepare a novel 3,3'-di(maleimide)-[1,1'-biphenyl]-4,4'-dicarboxylic acid as the first carboxylic acid monomer, and then uses DOPO-maleic acid as the second carboxylic acid monomer to carry out melt polycondensation reaction with 4,4'-(piperazine-1,4-diyl) diphenylamine to obtain a novel poly(biphenyl maleimide-DOPO-piperazine) flame retardant.

[0015] The present invention uses diisopropylbenzene peroxide or di-tert-butyl peroxide as an initiator, and the alkenyl maleimide group in the flame retardant can undergo grafting and crosslinking reaction with polyolefins such as polypropylene and polyethylene, thereby crosslinking and grafting polyaromatic amide polymers containing maleimide rings and biphenyl structures with high thermal decomposition properties to polyolefin molecular chains such as polypropylene, so that the crosslinked polypropylene has a higher initial decomposition temperature (temperature at which the mass loss is 5%) and better high temperature resistance. In addition, when the amount of flame retardant added is small, the tensile strength of the crosslinked polypropylene is significantly improved.

[0016] The poly(biphenyl maleimide-DOPO-piperazine) flame retardant of the present invention contains DOPO phosphate as an acid source, piperazine and maleimide nitrogen-containing heterocyclic rings as gas sources, and a large amount of biphenyl and aromatic ring fabric carbon sources to form an expansion flame retardant system. When burning, an expansion carbon layer is formed in a polyolefin matrix such as polypropylene, thereby significantly improving the limiting oxygen index and flame retardancy of the polyolefin. DETAILED DESCRIPTION

[0017] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only intended to illustrate the present invention and are not intended to limit the scope of the present invention. The operating methods in the following examples where no specific conditions are indicated are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0018] The preparation method of DOPO-maleic acid is as follows: add 100g toluene, 100g tetrahydrofuran, 162g DOPO, and 87g maleic acid into a reaction container, heat to 90°C, condense and reflux for 20h, filter after cooling, collect the filter cake, and obtain DOPO-maleic acid. The structural formula is

[0019] Example 1

[0020] Add 110 mL of N,N-dimethylformamide, 40 mmol of 3,3'-diamino-[1,1'-biphenyl]-4,4'-dicarboxylic acid, and 88 mmol of maleic anhydride to the reaction vessel, carry out acylation reaction at 35°C for 15 hours, concentrate under reduced pressure, wash the intermediate with acetone, add 150 mL of acetic anhydride after drying, and then add 50 mmol of sodium acetate, carry out cyclization reaction at 70°C for 4 hours, concentrate under reduced pressure, wash the product with water and acetone in turn, and dry it to obtain N-isophthalic acid maleimide. The preparation reaction formula is:

[0021]

[0022] Nitrogen was introduced into the reactor, 85 mmol DOPO-maleic acid, 100 mmol 4,4'-(piperazine-1,4-diyl) diphenylamine, and 15 mmol 3,3'-di(maleimide)-[1,1'-biphenyl]-4,4'-dicarboxylic acid were added, and melt polymerization was carried out at 260°C for 2 hours. After the reaction, the mixture was cooled, washed with ethanol, and dried to obtain a poly(biphenyl maleimide-DOPO-piperazine) flame retardant. The preparation reaction mechanism is as follows:

[0023]

[0024] 960g of polypropylene resin, 30g of poly(biphenylmaleimide-DOPO-piperazine) flame retardant, 2g of initiator di-tert-butyl peroxide, and 5g of antioxidant 1076 were added to a twin-screw extrusion rheometer with a screw speed of 60r / mn and a melt temperature of 220°C. The mixture was extruded and granulated to obtain a halogen-free flame retardant modified plastic masterbatch.

[0025] Example 2

[0026] 120 mL of N,N-dimethylformamide, 40 mmol of 3,3'-diamino-[1,1'-biphenyl]-4,4'-dicarboxylic acid and 96 mmol of maleic anhydride were added to the reaction container, and the acylation reaction was carried out at 20°C for 18 hours, and the mixture was concentrated under reduced pressure. The intermediate was washed with acetone, dried and added to 100 mL of acetic anhydride, and then 35 mmol of sodium acetate was added. The cyclization reaction was carried out at 60°C for 8 hours, and the mixture was concentrated under reduced pressure. The product was washed with water and acetone in turn, and dried to obtain N-isophthalic acid maleimide.

[0027] Nitrogen was introduced into the reactor, and 75 mmol DOPO-maleic acid, 100 mmol 4,4'-(piperazine-1,4-diyl)diphenylamine, and 25 mmol 3,3'-di(maleimide)-[1,1'-biphenyl]-4,4'-dicarboxylic acid were added. Melt polymerization was carried out at 270°C for 1 hour. After the reaction, the mixture was cooled, washed with ethanol, and dried to obtain a poly(biphenylmaleimide-DOPO-piperazine) flame retardant.

[0028] 900g of polypropylene resin, 90g of poly(biphenylmaleimide-DOPO-piperazine) flame retardant, 5g of initiator diisopropylbenzene peroxide, and 2g of antioxidant 1076 were added to a twin-screw extrusion rheometer with a screw speed of 150r / mn and a melting temperature of 220°C. The mixture was extruded and granulated to obtain a halogen-free flame retardant modified plastic masterbatch.

[0029] Example 3

[0030] 120 mL of N,N-dimethylformamide, 40 mmol of 3,3'-diamino-[1,1'-biphenyl]-4,4'-dicarboxylic acid and 96 mmol of maleic anhydride were added to the reaction container, and the acylation reaction was carried out at 30 ° C for 12 hours, and the reaction was concentrated under reduced pressure. The intermediate was washed with acetone, dried and added to 150 mL of acetic anhydride, and then 40 mmol of sodium acetate was added. The cyclization reaction was carried out at 60 ° C for 6 hours, and the reaction was concentrated under reduced pressure. The product was washed with water and acetone in turn, and dried to obtain N-isophthalic acid maleimide.

[0031] Nitrogen was introduced into the reactor, and 60 mmol DOPO-maleic acid, 100 mmol 4,4'-(piperazine-1,4-diyl)diphenylamine, and 40 mmol 3,3'-di(maleimide)-[1,1'-biphenyl]-4,4'-dicarboxylic acid were added. Melt polymerization was carried out at 260°C for 2 h. After the reaction, the mixture was cooled, washed with ethanol, and dried to obtain a poly(biphenylmaleimide-DOPO-piperazine) flame retardant.

[0032] 840g of polypropylene resin, 150g of poly(biphenylmaleimide-DOPO-piperazine) flame retardant, 8g of initiator di-tert-butyl oxide, and 2g of antioxidant 1076 were added to a twin-screw extrusion rheometer with a screw speed of 150r / mn and a melting temperature of 220°C. The mixture was extruded and granulated to obtain a halogen-free flame retardant modified plastic masterbatch.

[0033] Comparative Example 1

[0034] 960g of polypropylene resin, 2g of initiator di-tert-butyl peroxide, and 5g of antioxidant 1076 were added to a twin-screw extrusion rheometer. The screw speed was 60r / mn, the melting temperature was 220°C, and extrusion and granulation were performed to obtain polypropylene plastic masterbatch.

[0035] Comparative Example 2

[0036] Nitrogen was introduced into the reactor, 100 mmol 4,4'-(piperazine-1,4-diyl)diphenylamine and 100 mmol DOPO-maleic acid were added, and melt polymerization was carried out at 260°C for 2 h. After the reaction, the reactor was cooled, washed with ethanol, and dried to obtain a poly(DOPO-piperazine) flame retardant.

[0037] 960g of polypropylene resin, 30g of poly(DOPO-piperazine) flame retardant, 2g of initiator di-tert-butyl peroxide, and 5g of antioxidant 1076 were added to a twin-screw extrusion rheometer with a screw speed of 60r / mn and a melting temperature of 220°C. The mixture was extruded and granulated to obtain a halogen-free flame retardant modified plastic masterbatch.

[0038] Comparative Example 3

[0039] Nitrogen was introduced into the reactor, and 100 mmol 4,4'-(piperazine-1,4-diyl)diphenylamine and 100 mmol 3,3'-di(maleimide)-[1,1'-biphenyl]-4,4'-dicarboxylic acid (prepared according to the method of Example 1) were added, and melt polymerization was carried out at 260°C for 2 h. After the reaction, the mixture was cooled, washed with ethanol, and dried to obtain a poly(biphenylmaleimide-piperazine) flame retardant.

[0040] 960g of polypropylene resin, 30g of poly(biphenylmaleimide-piperazine) flame retardant, 2g of initiator di-tert-butyl peroxide, and 5g of antioxidant 1076 were added to a twin-screw extrusion rheometer with a screw speed of 60r / mn and a melt temperature of 220°C. The mixture was extruded and granulated to obtain a halogen-free flame retardant modified plastic masterbatch.

[0041] The halogen-free flame retardant modified plastic masterbatch was injection molded to make test specimens. The flame retardant properties of the test specimens were tested according to the GB / T 2406.1-2008 method. The tensile properties of the test specimens were tested according to the GB / T 1040.1-2006 method.

[0042] The thermal properties of the test specimens were tested using a thermogravimetric analyzer. The specimen size was 2 cm × 2 cm × 0.2 cm. The nitrogen atmosphere, heating rate was 10 °C / min, and the temperature range was 20-800 °C. The test results are shown in Table 1.

[0043] Table 1 Performance test of polypropylene plastic masterbatch

[0044]

[0045] Compared with the pure polypropylene plastic masterbatch of comparative example 1, poly(biphenyl maleimide-DOPO-piperazine) flame retardant is added in Examples 1, 2 and 3. The flame retardant contains DOPO phosphate as an acid source, piperazine and maleimide nitrogen-containing heterocyclic rings as gas sources, and a large amount of biphenyl and aromatic ring fabric carbon sources to form an expansion flame retardant system. When burning, an expansion carbon layer is formed in the polypropylene matrix, which improves the limiting oxygen index and flame retardancy of polypropylene. In addition, the flame retardant contains maleimide rings, and its alkenyl group undergoes a grafting reaction with polypropylene under the action of the initiator diisopropylbenzene peroxide or di-tert-butyl peroxide, thereby cross-linking and grafting the polyaromatic amide polymer flame retardant containing a highly thermally decomposable maleimide ring and a biphenyl structure into the polypropylene molecular chain, so that the cross-linked polypropylene has a higher initial decomposition temperature (temperature of 5% mass loss) and has better high temperature resistance. In addition, a small amount of poly(biphenyl maleimide-DOPO-piperazine) flame retardant was added in Examples 1 and 2, and the tensile strength of the cross-linked polypropylene was significantly improved.

[0046] In comparative example 2, when preparing the flame retardant, 3,3'-di(maleimide)-[1,1'-biphenyl]-4,4'-dicarboxylic acid was not added, and the obtained poly(DOPO-piperazine) flame retardant did not contain maleimide rings and could not undergo cross-linking reaction with polystyrene. Although the limiting oxygen index and flame retardant properties of polypropylene were significantly improved, the initial decomposition temperature and tensile strength were low.

[0047] In comparative example 3, when preparing the flame retardant, DOPO-maleic acid was not added, and the obtained poly(biphenyl maleimide-piperazine) flame retardant did not contain DOPO phosphate flame retardant groups, and the limiting oxygen index and flame retardant properties of polypropylene were poor. However, it contains polyaromatic amide and biphenyl maleimide high temperature resistant structure, and can be chemically cross-linked with polypropylene, and the initial decomposition temperature and tensile strength of polypropylene are significantly improved.

[0048] Example 4

[0049] 960 g of polypropylene resin, 30 g of poly(biphenylmaleimide-DOPO-piperazine) flame retardant (prepared according to the method of Example 1), 2 g of initiator di-tert-butyl peroxide, and 5 g of antioxidant 1076 were added to a twin-screw extrusion rheometer with a screw speed of 60 r / mn and a melt temperature of 220°C. The mixture was extruded and granulated to obtain a halogen-free flame retardant modified plastic masterbatch.

[0050] Comparative Example 4

[0051] 960g of polypropylene resin, 2g of initiator di-tert-butyl peroxide, and 5g of antioxidant 1076 were added to a twin-screw extrusion rheometer. The screw speed was 60r / mn, the melting temperature was 220°C, and extrusion and granulation were performed to obtain polypropylene plastic masterbatch.

[0052] Example 5

[0053] 960 g of polystyrene resin, 30 g of poly(biphenylmaleimide-DOPO-piperazine) flame retardant (prepared according to the method of Example 1), 2 g of initiator di-tert-butyl peroxide, and 5 g of antioxidant 1076 were added to a twin-screw extrusion rheometer with a screw speed of 60 r / mn and a melt temperature of 220°C. Extrusion and granulation were performed to obtain a halogen-free flame retardant modified plastic masterbatch.

[0054] Comparative Example 5

[0055] 960g of polystyrene resin, 2g of initiator di-tert-butyl peroxide, and 5g of antioxidant 1076 were added to a twin-screw extrusion rheometer with a screw speed of 60r / mn and a melting temperature of 220°C. The mixture was extruded and granulated to obtain a polystyrene plastic masterbatch.

[0056] Example 6

[0057] 960 g of polyvinyl chloride resin, 30 g of poly(biphenylmaleimide-DOPO-piperazine) flame retardant (prepared according to the method of Example 1), 2 g of initiator di-tert-butyl peroxide, and 5 g of antioxidant 1076 were added to a twin-screw extrusion rheometer with a screw speed of 60 r / mn and a melt temperature of 220°C. The mixture was extruded and granulated to obtain a halogen-free flame retardant modified plastic masterbatch.

[0058] Comparative Example 6

[0059] 960g of polyvinyl chloride resin, 2g of initiator di-tert-butyl peroxide, and 5g of antioxidant 1076 were added to a twin-screw extrusion rheometer. The screw speed was 60r / mn, the melting temperature was 220°C, and extrusion and granulation were performed to obtain polyvinyl chloride plastic masterbatch.

[0060] The plastic masterbatch was injection molded to make test specimens. The flame retardant properties of the test specimens were tested according to GB / T 2406.1-2008 and UL 94. The test results are shown in Table 2.

[0061] Table 2 Flame retardant properties test of plastic masterbatch

[0062] Limiting oxygen index (%) Example 4 27.3 Comparative Example 4 17.5 Example 5 28.0 Comparative Example 5 18.4 Example 6 28.2 Comparative Example 6 23.1

[0063] The poly(biphenyl maleimide-DOPO-piperazine) flame retardant prepared by the invention has excellent flame retardant performance to polyethylene, polystyrene and polyvinyl chloride.

[0064] In addition, it should be understood that after reading the above description of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A halogen-free flame retardant modified plastic masterbatch, characterized in that: The halogen-free flame retardant modified plastic masterbatch comprises the following components: 84-96 parts by weight of polyolefin resin, 3-15 parts by weight of poly(biphenyl maleimide-DOPO-piperazine) flame retardant, 0.2-0.8 parts by weight of initiator, and 0.2-0.5 parts by weight of antioxidant; The preparation method of the poly(biphenyl maleimide-DOPO-piperazine) flame retardant is as follows: nitrogen is introduced into a reaction kettle, 4,4'-(piperazine-1,4-diyl) diphenylamine, DOPO-maleic acid, and 3,3'-di(maleimide)-[1,1'-biphenyl]-4,4'-dicarboxylic acid are added, melt polymerization is performed, cooling is performed after the reaction, washing with ethanol, and drying is performed to obtain the poly(biphenyl maleimide-DOPO-piperazine) flame retardant; The ratio of the 4,4'-(piperazine-1,4-diyl)diphenylamine, DOPO-maleic acid, and 3,3'-di(maleimide)-[1,1'-biphenyl]-4,4'-dicarboxylic acid is 1 mol: (0.6-0.85) mol: (0.15-0.4) mol; The preparation method of 3,3'-di(maleimide)-[1,1'-biphenyl]-4,4'-dicarboxylic acid is as follows: N,N-dimethylformamide, 3,3'-diamino-[1,1'-biphenyl]-4,4'-dicarboxylic acid and maleic anhydride are added to a reaction container to perform an acylation reaction, and the reaction is concentrated under reduced pressure. The intermediate is washed with acetone, dried and then added to acetic anhydride, and then sodium acetate is added to perform a cyclization reaction, and the reaction is concentrated under reduced pressure. The product is washed with water and acetone in turn and dried to obtain 3,3'-di(maleimide)-[1,1'-biphenyl]-4,4'-dicarboxylic acid. The ratio of the 3,3'-diamino-[1,1'-biphenyl]-4,4'-dicarboxylic acid to maleic anhydride is 1 mol:(2.2-2.4) mol.

2. The halogen-free flame retardant modified plastic masterbatch according to claim 1, characterized in that: The polyolefin resin includes at least one of polypropylene, polyethylene and polystyrene.

3. The halogen-free flame retardant modified plastic masterbatch according to claim 1, characterized in that: The initiator is at least one of dicumyl peroxide and di-tert-butyl peroxide.

4. The halogen-free flame retardant modified plastic masterbatch according to claim 1, characterized in that: The melt polymerization is controlled at a temperature of 260-270° C. and a time of 1-2 hours.

5. The halogen-free flame retardant modified plastic masterbatch according to claim 1, characterized in that: The acylation reaction is controlled at a temperature of 20-35° C. and a time of 12-18 h.

6. The halogen-free flame retardant modified plastic masterbatch according to claim 1, characterized in that: The cyclization reaction is controlled at a temperature of 60-70° C. and a time of 4-8 hours.

7. A method for preparing a halogen-free flame retardant modified plastic masterbatch according to any one of claims 1 to 6, characterized in that: The preparation method is as follows: polyolefin resin, poly(biphenyl maleimide-DOPO-piperazine) flame retardant, initiator and antioxidant are added into a twin-screw extrusion rheometer, the screw speed is 60-150r / min, extrusion and granulation are performed to obtain halogen-free flame retardant modified plastic masterbatch.