Carbon fiber composite material for bicycle frame and preparation method thereof

By using carbon fiber composite materials impregnated with epoxy resin on the bicycle frame, the problem of strong vibration and poor impact resistance of the bicycle frame on rough roads is solved, achieving high strength, impact resistance, shock absorption and scratch resistance. damage performance, simplifying the production process and reducing costs.

CN118344719BActive Publication Date: 2024-10-15惠州市德泰士达科技有限公司
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410500257.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-24
Publication Date
2024-10-15
Estimated Expiration
2044-04-24

AI Technical Summary

Technical Problem

Existing bicycle frame materials have strong vibrations on rough roads, poor impact resistance, and are easily scratched by stones and branches. The production efficiency is low, the price is high, and the scratch resistance is insufficient.

Method used

Using carbon fiber composite materials, by impregnating the carbon fiber with epoxy resin and combining it with polycarbonate resin, polyformaldehyde resin, compatibilizer, lubricant and light stabilizer, a carbon fiber composite material with a bimodal fiber length distribution is prepared. , improve its dispersion and scratch resistance.

Benefits of technology

It achieves high strength, high impact shock absorption and scratch resistance, simplifies the production process, improves the uniformity and comprehensive performance of the material, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004808444620000061
    Figure BDA0004808444620000061
  • Figure BDA0004808444620000071
    Figure BDA0004808444620000071
  • Figure BDA0004808444620000072
    Figure BDA0004808444620000072
Patent Text Reader

Abstract

The invention discloses a carbon fiber composite material applied to a bicycle frame and a preparation method thereof, belonging to the technical field of modified plastics, the carbon fiber composite material of the invention comprises the following components by weight: 50-80 parts of polycarbonate resin, 20-50 parts of polyoxymethylene resin, 15-60 parts of carbon fiber, 5-10 parts of compatibilizer, 0.1-2 parts of lubricant, 0.1-2 parts of light stabilizer, the fiber length distribution of the carbon fiber in the composite material is a bimodal distribution, including a first wave peak of 3-5mm in fiber length and a second wave peak of 7-10mm in fiber length, the peak area ratio of the first wave peak to the second wave peak is 1:(0.5-2), and the carbon fiber is a carbon fiber with a surface treated with epoxy resin impregnation. The carbon fiber composite material prepared by the present invention has the advantages of high strength, high impact resistance, scratch resistance, easy processing, etc., and can be used to make a high-performance, lightweight bicycle frame.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a carbon fiber composite material applied to a bicycle frame and a preparation method thereof. Background Art

[0002] Cycling is an aerobic sport that is loved by people. One of the key criteria for selecting sports bicycles is that the frame must meet the conditions of light weight, sufficient strength, and high rigidity. At present, the frame materials of commercially available sports bicycles are generally aluminum alloy, carbon fiber, titanium alloy and alloy steel. The alloy material has good rigidity, but poor impact resistance, strong vibration when riding on rugged roads, and not light enough. Carbon fiber frame has the advantages of high strength, light weight and high plasticity, strong buffering effect, stable riding feeling and light weight when riding, and its advantages are best reflected when climbing. Carbon fiber can be used to make frames of various shapes. The general basic molding method is to lay fiber sheets on the mold and then flow into resin and burn it, but this method requires a large amount of carbon fiber material, which is expensive, and it is necessary to manually stick the carbon fiber cloth to the mold piece by piece during production, which is inefficient. In addition, bicycles are often prone to scratches from stones and branches when riding on mountain roads, which affects the beauty of the vehicle, and the existing technology rarely involves the problem of scratch resistance of bicycle frames. Summary of the invention

[0003] In order to overcome the deficiencies of the prior art, the present invention provides a carbon fiber composite material for a bicycle frame, which has the characteristics of high strength, high impact resistance and shock absorption, good scratch resistance and the like.

[0004] Another object of the present invention is to provide a method for preparing a carbon fiber composite material for a bicycle frame.

[0005] The present invention is achieved through the following technical scheme: a carbon fiber composite material applied to a bicycle frame, comprising the following components by weight: 50-80 parts of polycarbonate resin, 20-50 parts of polyoxymethylene resin, 15-60 parts of carbon fiber, 5-10 parts of compatibilizer, 0.1-2 parts of lubricant, and 0.1-2 parts of light stabilizer. The fiber length distribution of the carbon fiber in the composite material is a bimodal distribution, comprising a first wave peak with a fiber length of 3-5 mm and a second wave peak with a fiber length of 7-10 mm. The peak area ratio of the first wave peak to the second wave peak is 1:(0.5-2). The carbon fiber is a carbon fiber whose surface is impregnated with epoxy resin.

[0006] Carbon fibers with longer fiber lengths have better tensile and impact properties, but poorer dispersion and wettability. When used with carbon fibers with shorter fiber lengths, the dispersion of the carbon fibers in the composite material can be improved, making the composite material more uniform. At the same time, short carbon fibers form a finer microstructure in the composite material, which helps to improve the scratch resistance of the material.

[0007] At the same time, the carbon fiber surface has low chemical activity and few physical bonding points, which makes it difficult to meet the requirements of interface construction of carbon fiber composite materials. The present invention uses epoxy resin to impregnate the carbon fiber surface, which can further improve the comprehensive performance of the carbon fiber composite material.

[0008] In a specific embodiment, the mass of the epoxy resin is 50wt%-200wt% of the mass of the carbon fiber. Preferably, the mass of the epoxy resin is 80wt%-120wt% of the mass of the carbon fiber.

[0009] In a specific embodiment, the melt mass flow rate of the polyoxymethylene resin at 190°C and 2.16 kg is 2-25 g / 10 min. Preferably, the melt mass flow rate of the polyoxymethylene resin at 190°C and 2.16 kg is 7-15 g / 10 min. The melt flow rate of the polyoxymethylene resin can be measured according to ISO 1133-1:2011.

[0010] In a specific embodiment, the epoxy value of the epoxy resin is 0.3-0.8, preferably, the epoxy value of the epoxy resin is 0.4-0.6; the epoxy value of the epoxy resin is obtained by titration using hydrochloric acid-acetone titration method according to GB / T1677-2008.

[0011] In a specific embodiment, the melt flow rate of the polycarbonate under the test conditions of 300° C. and 1.2 kg is 10-22 g / 10 min, and the melt flow rate of the polycarbonate is measured with reference to ISO 1133-1-2011.

[0012] In a specific embodiment, the compatibilizer is a glycidyl methacrylate graft and / or a maleic anhydride graft. Preferably, the compatibilizer is a glycidyl methacrylate graft. Further preferably, the glycidyl methacrylate graft is one or more of glycidyl methacrylate grafted ethylene-octene copolymer (POE-g-GMA), glycidyl methacrylate grafted ethylene-methyl acrylate copolymer (EMA-g-GMA), glycidyl methacrylate grafted hydrogenated styrene-butadiene block copolymer (SEBS-g-GMA), glycidyl methacrylate grafted ethylene-propylene rubber (EPDM-g-GMA), and glycidyl methacrylate grafted styrene resin, and the maleic anhydride graft is one or more of maleic anhydride grafted ethylene-octene copolymer, maleic anhydride grafted ABS, maleic anhydride grafted polystyrene or maleic anhydride grafted AS.

[0013] In a specific embodiment, the lubricant is selected from one or more of polyethylene wax, polyol ester or stearate, and the light stabilizer is selected from one or more of hindered amine light stabilizers, benzotriazole light stabilizers, benzophenone light stabilizers or hindered benzoate light stabilizers.

[0014] In a specific embodiment, the carbon fiber composite material further includes one or more of a colorant, a dye, an ultraviolet absorber, and an antioxidant.

[0015] The present invention also protects a method for preparing a carbon fiber composite material for a bicycle frame, comprising the following steps: (1) pretreatment: drying a polycarbonate resin and a polyoxymethylene resin at 80-120°C for 3-8 hours for standby use, and impregnating the carbon fiber with epoxy resin and then curing it for 3-8 hours for standby use; (2) weighing each component according to a proportion, and sequentially putting the polycarbonate resin, polyoxymethylene resin, carbon fiber, compatibilizer, lubricant, and light stabilizer into a premixer for mixing; (3) putting the mixed material into a twin-screw extruder, the extrusion screw aspect ratio is 30:1-40:1, the extruder temperature is set at 100-140°C in the T1 zone, 230-250°C in the T2-T5 zone, and 250-260°C in the T6-T12 zone, and the rotation speed is 300-450r / min, and the carbon fiber composite material is obtained by mixing, melting, homogenizing, and then extruding and granulating.

[0016] Preferably, in step (1), the curing agent used for curing the carbon fiber after impregnation with epoxy resin is selected from any one or more of diethyltoluenediamine, N,N-dimethylformamide, and diaminodiphenyl sulfone.

[0017] Beneficial Effects

[0018] The present invention provides a carbon fiber composite material for a bicycle frame, wherein the carbon fiber is impregnated with epoxy resin and then mixed with PC resin, POM resin, compatibilizer, lubricant, light stabilizer, etc., and extruded and granulated to obtain a carbon fiber composite material suitable for a bicycle frame. The carbon fiber composite material of the present invention can be injection molded in various bicycle molds to obtain an integrated bicycle frame, and the overall structure of the frame has no welding points, thereby avoiding the problem of weak welding points of traditional metal alloys. In addition, the injection molding process is simple, the mold can be reused, and the production efficiency is improved.

[0019] The carbon fiber composite material prepared by the present invention by screening carbon fibers with a specific fiber length combination meets the characteristics of high strength, high impact resistance and scratch resistance. At the same time, the carbon fiber is pre-impregnated with epoxy resin and the addition of a compatibilizer can improve the compatibility of the carbon fiber with PC and POM resins, making the carbon fiber composite material more uniform and having a high qualified rate of finished products. DETAILED DESCRIPTION

[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] In the examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.

[0022] The raw materials used in the embodiments and comparative examples are described as follows:

[0023] Polycarbonate resin 1: melt mass flow rate 10 g / 10 min, PC1300-10NP, LG Chem;

[0024] Polycarbonate resin 2: melt mass flow rate 22 g / 10 min, PC1300-22NP, LG Chem;

[0025] Polycarbonate resin 3: melt mass flow rate 3 g / 10 min, PC1300-03NP, LG Chem;

[0026] Polyoxymethylene resin 1: melt mass flow rate 25g / 10min, FG900PNC010, DuPont;

[0027] Polyoxymethylene resin 2: melt mass flow rate 15g / 10min, FG500PNC010, DuPont;

[0028] Polyoxymethylene resin 3: melt mass flow rate 7g / 10min, FG311DPNC010, DuPont;

[0029] Polyoxymethylene resin 4: melt mass flow rate 2.3g / 10min, FG150NC010, DuPont;

[0030] Carbon fiber 1: Fiber length is 3-5mm, purchased from Shuobang New Materials, Fuzhou, Jiangxi

[0031] Carbon fiber 2: fiber length is 7-10mm, purchased from Shuobang New Materials, Fuzhou, Jiangxi

[0032] The carbon fiber is obtained by further screening carbon fiber raw materials with a length of 1-10 mm.

[0033] Epoxy resin 1: bisphenol A epoxy resin, CYD-134, epoxy value 0.38, Sinopec;

[0034] Epoxy resin 2: diglycidyl ether bisphenol A epoxy resin, KE-133L, epoxy value 0.55, Chengdu KEMMET;

[0035] Epoxy resin 3: ethylene glycol diglycidyl ether, industrial grade, epoxy value 0.7, Foshan Hongshuo Chemical;

[0036] Epoxy resin 4: 2-epoxyhexane-4,5-dicarboxylic acid diglycidyl ester, TDE-85, epoxy value 0.85, Tianjin Jingdong;

[0037] Curing agent: diethyltoluenediamine, purity> 99%, Sinopharm Chemical Reagent Co., Ltd.;

[0038] Compatibilizer 1: glycidyl methacrylate grafted compound, specifically POE-g-GMA, SOG-03, Jiayirong;

[0039] Compatibilizer 2: glycidyl methacrylate grafted product, specifically glycidyl methacrylate grafted ethylene-methyl acrylate copolymer, KT-33, Shenyang Ketong Plastic Co., Ltd.;

[0040] Compatibilizer 3: glycidyl methacrylate grafted product, specifically maleic anhydride grafted ethylene-octene copolymer, Fusabond N493, DuPont;

[0041] Lubricant: polyethylene wax, commercially available;

[0042] Light stabilizer: TINUVIN234, commercially available.

[0043] Unless otherwise specified, the components and raw materials used in the embodiments and comparative examples of the present invention are all commercially available raw materials, and the components and raw materials used in each parallel experiment are all of the same kind.

[0044] Example 1-19 A carbon fiber composite material and a method for preparing the same

[0045] Embodiment 1-19 provides a carbon fiber composite material and a preparation method thereof. The weight formula thereof is shown in Table 1. The preparation method is as follows:

[0046] 1) Pretreatment: drying the polycarbonate resin and the polyoxymethylene resin at 100°C for 6 hours, and impregnating the carbon fiber with epoxy resin and curing it for 6 hours;

[0047] 2) Weigh each component according to the ratio, and sequentially put the polycarbonate resin, polyoxymethylene resin, carbon fiber, compatibilizer, lubricant, and light stabilizer into a premixer for mixing.

[0048] 3) The mixed material is put into a twin-screw extruder, the aspect ratio of the extrusion screw is 30:1-40:1, the temperature of the extruder is set at 100-140°C in the T1 zone, 230-250°C in the T2-T5 zone, 250-260°C in the T6-T12 zone, and the speed is 300-450r / min. The carbon fiber composite material is obtained by extrusion granulation after mixing, melting, and homogenization.

[0049] Table 1

[0050]

[0051] Table 1

[0052]

[0053] The preparation method of Comparative Example 1-6 is the same as that of Example 1-19, and the weight formula is shown in Table 2. The carbon fiber of Comparative Example 7 is not impregnated with epoxy resin, and the rest is the same as that of Example 1-19.

[0054] Table 2

[0055]

[0056]

[0057] The carbon fiber composite materials prepared in Examples 1-19 and Comparative Examples 1-7 were subjected to the following performance tests, and the results are shown in Table 3.

[0058] 1. Tensile strength: According to ISO527-2-2012 standard, the sample is injection molded into 1A type tensile specimen for testing; test conditions: tensile rate 10mm / min, 23℃.

[0059] 2. Impact strength: The products of the embodiments and comparative examples were subjected to cantilever beam notched impact test, A-type notch, according to ISO180-2000 standard;

[0060] 3. Scratch resistance: Use a cross scratch tester to test the injection molded sample, with a scratch load of 10N. The scratch resistance of the material is judged based on the color difference ΔL before and after the scratch. The lower the ΔL value, the harder it is to find the scratch, and the better the scratch resistance. For scratch-resistant materials, the ΔL value before and after the scratch is usually required to be less than 1.5.

[0061] Table 3

[0062]

[0063]

[0064] The present invention provides a carbon fiber composite material for a bicycle frame, the tensile strength of which is ≥108MPa and the impact strength of which is ≥27.7KJ / m 2 , scratch resistance ΔL≥1.34, meeting the frame application requirements of various bicycles.

[0065] It can be seen from Examples 3-5, Comparative Examples 1-2, and Comparative Examples 5-6 that by selecting a carbon fiber combination with a specific fiber length distribution, the carbon fiber composite material has good tensile strength, impact resistance, and scratch resistance, which meets the requirements of high strength, impact resistance, and shock absorption of sports bicycles and has a scratch resistance effect.

[0066] From Examples 3, 6-9, and Comparative Example 7, it can be seen that the use of epoxy resin to impregnate the surface of carbon fiber can improve the tensile strength, impact resistance, and scratch resistance of the carbon fiber composite material, and when the mass of the epoxy resin is 80wt%-120wt% of the mass of the carbon fiber, the comprehensive effect is the best. In addition, the epoxy value of the epoxy resin also has a significant effect on the performance of the carbon fiber composite material. When the epoxy value of the epoxy resin is 0.4-0.6, the tensile strength, impact resistance, and scratch resistance of the carbon fiber composite material are better.

[0067] It can be seen from Examples 3, 10-11, and 12-14 that by selecting a polycarbonate with a melt flow rate of 10-22 g / 10 min under the test conditions of 300°C and 1.2 kg and a polyoxymethylene resin with a melt mass flow rate of 7-15 g / 10 min under the test conditions of 190°C and 2.16 kg, the carbon fiber composite material has better tensile strength, impact resistance, and scratch resistance.

[0068] It can be seen from Examples 3 and 18-19 that when glycidyl methacrylate grafts are used as compatibilizers, the comprehensive performance of the carbon fiber composite material is better than that of maleic anhydride grafts.

[0069] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A carbon fiber composite material for a bicycle frame, It is characterized in that The composite material comprises the following components by weight: 50-80 parts of polycarbonate resin, 20-50 parts of polyoxymethylene resin, 15-60 parts of carbon fiber, 5-10 parts of compatibilizer, 0.1-2 parts of lubricant and 0.1-2 parts of light stabilizer. The fiber length distribution of the carbon fiber in the composite material is a bimodal distribution, including a first peak with a fiber length of 3-5 mm and a second peak with a fiber length of 7-10 mm. The peak area ratio of the first peak to the second peak is 1:(0.5-2). The carbon fiber is a carbon fiber whose surface is impregnated with epoxy resin.

2. The carbon fiber composite material according to claim 1, It is characterized in that The mass of the epoxy resin is 50wt%-200wt% of the mass of the carbon fiber.

3. The carbon fiber composite material according to claim 1, It is characterized in that The melt mass flow rate of the polyoxymethylene resin at 190° C. and 2.16 kg is 2-25 g / 10 min.

4. The carbon fiber composite material according to claim 1, It is characterized in that The epoxy value of the epoxy resin is 0.3-0.

8.

5. The carbon fiber composite material according to claim 1, It is characterized in that The polycarbonate has a melt flow rate of 10-22 g / 10 min under the test conditions of 300° C. and 1.2 kg.

6. The carbon fiber composite material according to claim 1, It is characterized in that The compatibilizer is a glycidyl methacrylate graft and / or a maleic anhydride graft.

7. The carbon fiber composite material according to claim 6, It is characterized in that The glycidyl methacrylate grafted material is one or more of glycidyl methacrylate grafted ethylene-octene copolymer, glycidyl methacrylate grafted ethylene-methyl acrylate copolymer, glycidyl methacrylate grafted hydrogenated styrene-butadiene block copolymer, glycidyl methacrylate grafted EPDM rubber, and glycidyl methacrylate grafted styrene resin; the maleic anhydride grafted material is one or more of maleic anhydride grafted ethylene-octene copolymer, maleic anhydride grafted ABS, maleic anhydride grafted polystyrene, or maleic anhydride grafted AS.

8. The carbon fiber composite material according to claim 1, It is characterized in that The lubricant is selected from one or more of polyethylene wax, polyol ester or stearate, and the light stabilizer is selected from one or more of hindered amine light stabilizers, benzotriazole light stabilizers, benzophenone light stabilizers or hindered benzoate light stabilizers.

9. The carbon fiber composite material according to claim 1, It is characterized in that The carbon fiber composite material also includes one or more of a colorant, an ultraviolet absorber, and an antioxidant.

10. The method for preparing the carbon fiber composite material according to any one of claims 1 to 8, It is characterized in that The following steps are involved: (1) Pretreatment: drying the polycarbonate resin and polyoxymethylene resin at 80-120°C for 3-8 hours for later use, and impregnating the carbon fiber with epoxy resin and curing it for 3-8 hours for later use; (2) weighing each component according to the ratio, and sequentially putting the polycarbonate resin, polyoxymethylene resin, carbon fiber, compatibilizer, lubricant, and light stabilizer into a premixer for mixing; (3) putting the mixed material into a twin-screw extruder, the extrusion screw aspect ratio is 30:1-40:1, the extruder temperature is set at 100-140°C in the T1 zone, 230-250°C in the T2-T5 zone, and 250-260°C in the T6-T12 zone, and the speed is 300-450r / min. The carbon fiber composite material is obtained by mixing, melting, homogenizing, and then extruding and granulating.

Citation Information

Patent Citations

  • Halogen-free flame retardant cold-resistant conductive polycarbonate / carbon fiber composite material and preparation method thereof

    CN103525052A

  • Carbon fiber reinforced polyamide composite material pre-infiltrated basalt fiber cloth and preparation method thereof

    CN111057369A

  • Carbon fiber reinforced weather-proof PC / ASA composite material and preparation method thereof

    CN111320854A

  • Resin composition for resin molding, and resin molding

    EP3378888A1

  • Fiber-reinforced thermoplastic resin molding and fiber-reinforced thermoplastic resin molding material

    JP2015178610A