A preparation method of nitrogen-doped carbon quantum dots and application of carbon quantum dots in epoxy resin
Through the preparation and modification of epoxy resin by nitrogen-doped carbon quantum dots, the problem of limited application range of epoxy resin modified materials in the prior art is solved, and the rapid curing and high performance of epoxy resin is achieved, and thermal stability is achieved. and high temperature resistance.
Patent Information
- Application Number
- CN202410462212.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-17
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-04-17
AI Technical Summary
In the prior art, there are no reports on carbon quantum dots in modified materials of epoxy resin, which limits its application range. Low-molecular organic epoxy compounds do not have application value at room temperature, and need to be added to form cross-sections after adding curing agent. Only when connecting to the network is useful, but this process is complicated and lacks high-performance curing agents.
A nitrogen-doped carbon quantum dot preparation method is adopted. After ultrasonication of starch and triethylenetetramine in double-distilled water, it reacts in an autoclave, and combines microwave and cooling treatment to obtain purified nitrogen-doped carbon quantum dots. , and use it to modify epoxy resin to form nanoepoxy resins, achieving rapid curing and high performance.
It realizes rapid curing of epoxy resin (less than 10 minutes), has the advantage of rapid curing at room temperature, and improves the thermal stability and high-temperature reactivity of cured epoxy resin, providing high-performance epoxy resin materials.
Smart Images

Figure CN118344868B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of carbon nanomaterials, and in particular relates to a preparation method and application of nitrogen-doped carbon quantum dots. Background Art
[0002] Carbon quantum dots are the most eye-catching carbon nanomaterials after fullerenes, carbon nanotubes and graphene. They have attracted extensive attention from researchers because of their excellent optical properties, easy modification, and high biocompatibility. Carbon quantum dots have a wide range of raw material sources, low preparation costs, and the potential for large-scale production. They have good application prospects in many fields such as materials, chemical analysis, catalysis, and energy. In recent years, carbon quantum dots have made certain progress in material modification. CN202210498264 discloses a carbon quantum dot composite powder modified water-based coating and a preparation method thereof, which solves the technical problems of poor mechanics, storage stability, and UV resistance of water-based coatings in the prior art, and realizes a carbon quantum dot composite powder modified water-based coating with high hardness, excellent mechanical properties, and excellent dispersion stability. Fully exploring the advantages of carbon quantum dots and applying them to a wider range of material fields is the focus of future development.
[0003] Epoxy resin is a type of high molecular polymer containing two or more epoxy groups in its molecular structure. It is widely used in coatings, electronic packaging materials, composite materials and other fields because of its excellent thermal stability, chemical stability, electrical insulation, adhesion and chemical corrosion resistance. Low molecular weight organic epoxy compounds are in liquid or solid state at room temperature, have no application value, and cannot be directly used as structural or functional materials. Only after adding a curing agent to form a three-dimensional structure with a cross-linked network, it has use value. The properties of the curing agent determine the use direction and application value of the epoxy resin. Therefore, the development of high-performance epoxy curing agents has become the focus of research in this field. In recent years, various substances used for epoxy modification have emerged in an endless stream, greatly expanding the scope of application of epoxy resins, but modified materials based on carbon quantum dots have never been reported. In view of this, the development of ideal carbon quantum dots for epoxy resin modification has broad application prospects. Summary of the invention
[0004] The invention aims to provide a preparation and application of nano material-based epoxy resin to realize the development of nano epoxy resin, belonging to the technical field of epoxy resin.
[0005] In order to realize the above application, the present invention specifically provides the following technical solutions:
[0006] A method for preparing nitrogen-doped carbon quantum dots comprises the following steps:
[0007] Step 1, dissolving starch and triethylenetetramine in double distilled water, and ultrasonicating for 30 minutes to obtain a mixed solution;
[0008] Step 2, microwave the mixed solution for 5 minutes, then cool it and transfer it to a polytetrafluoroethylene-lined autoclave for reaction;
[0009] Step 3, cooling the yellow solution obtained by the reaction, centrifuging to remove precipitates and impurities, filtering with a 0.22 μm filter membrane, and then performing column chromatography to obtain a purified liquid;
[0010] Step 4: Freeze-dry the purified liquid under vacuum conditions to obtain a yellow solid powder, which is N-doped carbon quantum dots. The nitrogen-doped carbon quantum dots are configured into a 1.0 mg / mL aqueous solution and stored in a refrigerator at 4°C for later use.
[0011] In a specific implementation scheme, in step 1, pre-weighed starch and TETA are added to double distilled water in sequence, and the mass ratio of the starch to triethylenetetramine is 1:1 to 1:5; the mass volume ratio of the starch to double distilled water is 1:15.1:25.
[0012] In a specific embodiment, in step 2, the reaction temperature is 150-200° C., and the reaction time is 4-6 hours.
[0013] In a specific implementation manner, in step 3, the cooling temperature is -40 to -60°C.
[0014] In a specific implementation scheme, in step 3, the chromatography column developing agent is ethanol: water = 1:1.
[0015] In a specific embodiment, the particle size of the nitrogen-doped carbon quantum dots is 4.28±0.5 nm.
[0016] In a specific embodiment, nitrogen-doped carbon quantum dots are used in epoxy resin.
[0017] Compared with the prior art, the present invention has the following advantages:
[0018] 1. The raw materials for preparing the carbon quantum dots described in the present invention are abundant in source and low in price, and have the prospect of large-scale production.
[0019] 2. The carbon quantum dot curing agent of the present invention has the advantages of rapid curing (less than 10 minutes) at room temperature, and the cured epoxy resin has thermal stability and high temperature reactivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a schematic diagram of the structure of nitrogen-doped carbon quantum dots described in Example 1 of the present invention;
[0021] Figure 2 This is a transmission electron microscope image of the nitrogen-doped carbon quantum dots of the present invention;
[0022] Figure 3 This is a Fourier infrared spectrum of the nitrogen-doped carbon quantum dots of the present invention;
[0023] Figure 4 X-photoelectron spectrum of nitrogen-doped carbon quantum dots;
[0024] Figure 5 The epoxy resin form after curing of the present invention;
[0025] Figure 6 is the DSC curve of the epoxy resin of the present invention;
[0026] Figure 7 is the TG curve of the epoxy resin of the present invention; DETAILED DESCRIPTION
[0027] The present invention will be further explained below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the following specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.
[0028] The preparation method of nitrogen-doped carbon quantum dots of the present application comprises the following steps:
[0029] Step 1, starch and triethylenetetramine are dissolved in double distilled water, and ultrasonicated for 30 minutes to obtain a mixed solution;
[0030] Step 2, the mixed solution is transferred to a polytetrafluoroethylene-lined autoclave and reacted at 150-200° C. for 4-6 hours;
[0031] Step 3: The above product is post-processed by filtering with a 0.22 μm filter membrane and then performing column chromatography to obtain the product.
[0032] As a preferred embodiment of the present application, the preparation method of the nitrogen-doped carbon quantum dot-modified epoxy resin is:
[0033] Weigh 10-40 parts of epoxy resin, add 1-3 parts of curing agent, heat to 80-120° C., react for 2-5 hours, stir, and stand to obtain nano epoxy resin.
[0034] The schematic structural formula of the curing agent of the present application is:
[0035]
[0036] Example 1
[0037] A preparation method of nitrogen-doped carbon quantum dots N-CDs, the synthesis process is as follows Figure 1 As shown, the specific steps are as follows:
[0038] (1) Weigh 5.0201 g starch and 0.1 g triethylenetetramine, dissolve in 15 mL double distilled water, and sonicate for 30 minutes;
[0039] (2) placing the mixed solution in a microwave reactor and heating it for 5 minutes;
[0040] (3) The mixture solution was transferred to a 100 mL polytetrafluoroethylene-lined autoclave, and the autoclave was placed in an environment of 150° C. for reaction for 5 hours;
[0041] (4) The yellow solution obtained by the reaction was cooled to room temperature, then centrifuged for 25 minutes to remove large particles, filtered with a 0.22 μm filter membrane, and then subjected to column chromatography (developing solvent ethanol: water = 1:1) to obtain a pure product;
[0042] (5) Finally, the purified liquid is freeze-dried under vacuum conditions at -50°C to obtain nitrogen-doped carbon quantum dots.
[0043] Example 2
[0044] A preparation method of nitrogen-doped carbon quantum dots N-CDs, the synthesis process is as follows Figure 1 As shown, the specific steps are as follows:
[0045] (1) Weigh 5.0201 g starch and 0.2 g triethylenetetramine, dissolve in 15 mL double distilled water, and sonicate for 30 minutes;
[0046] (2) placing the mixed solution in a microwave reactor and heating it for 5 minutes;
[0047] (3) The mixture solution was transferred to a 100 mL polytetrafluoroethylene-lined autoclave, and the autoclave was placed in an environment of 160° C. for reaction for 5 hours;
[0048] (4) The yellow solution obtained by the reaction was cooled to room temperature, then centrifuged for 25 minutes to remove large particles, filtered with a 0.22 μm filter membrane, and then subjected to column chromatography (developing solvent ethanol: water = 1:1) to obtain a pure product;
[0049] (5) Finally, the purified liquid is freeze-dried under vacuum conditions at -50°C to obtain nitrogen-doped carbon quantum dots.
[0050] Example 3
[0051] A preparation method of nitrogen-doped carbon quantum dots N-CDs, the synthesis process is as follows Figure 1 As shown, the specific steps are as follows:
[0052] (1) Weigh 5.0201 g starch and 0.4 g triethylenetetramine, dissolve in 15 mL double distilled water, and sonicate for 30 minutes;
[0053] (2) placing the mixed solution in a microwave reactor and heating it for 5 minutes;
[0054] (3) The mixture solution was then transferred to a 100 mL polytetrafluoroethylene-lined autoclave, and the autoclave was placed in an environment of 180° C. for reaction for 5 hours;
[0055] (4) The yellow solution obtained by the reaction was cooled to room temperature, then centrifuged for 25 minutes to remove large particles, filtered with a 0.22 μm filter membrane, and then subjected to column chromatography (developing solvent ethanol: water = 1:1) to obtain a pure product;
[0056] (5) Finally, the purified liquid is freeze-dried under vacuum conditions at -50°C to obtain nitrogen-doped carbon quantum dots.
[0057] Example 4
[0058] A preparation method of nitrogen-doped carbon quantum dots N-CDs, the synthesis process is as follows Figure 1 As shown, the specific steps are as follows:
[0059] (1) Weigh 5.0201 g starch and 0.8 g triethylenetetramine, dissolve in 15 mL double distilled water, and sonicate for 30 minutes;
[0060] (2) placing the mixed solution in a microwave reactor and heating it for 5 minutes;
[0061] (3) The mixture solution was transferred into a 100 mL polytetrafluoroethylene-lined autoclave, and the autoclave was placed in an environment of 200° C. for reaction for 5 hours;
[0062] (4) The yellow solution obtained by the reaction was cooled to room temperature, then centrifuged for 25 minutes to remove large particles, filtered with a 0.22 μm filter membrane, and then subjected to column chromatography (developing solvent ethanol: water = 1:1) to obtain a pure product;
[0063] (5) Finally, the purified liquid is freeze-dried under vacuum conditions at -50°C to obtain nitrogen-doped carbon quantum dots.
[0064] Example 5
[0065] Figure 2 The transmission electron microscope TEM image and particle size distribution histogram of nitrogen-doped carbon quantum dots N-CDs show that spherical nanoparticles can be observed in the range of 1.72 to 9.68 nm, with an average size of 4.69 ± 0.4 nm. Clear lattice fringes with a spacing of 0.25 nm were observed in the HRTEM image, which is very similar to the lattice in the (100) plane of graphite, indicating that the nitrogen-doped carbon quantum dots have excellent crystallinity.
[0066] Figure 3This is the infrared spectrum of nitrogen-doped carbon quantum dots N-CDs. It can be seen from the figure that at 3415,3139cm -1 The characteristic absorption peak at 1652 cm is the OH / NH stretching vibration. -1 The characteristic absorption peak at 1400cm belongs to C=O stretching vibration, and the characteristic absorption peak is OH / NH stretching vibration. -1 Corresponds to the stretching vibration of CN. In addition, 1124cm -1 The peak at can be attributed to the stretching vibration of C-OH. This shows that the surface of the carbon quantum dots contains hydroxyl, carboxyl, carbonyl and amino groups, indicating that the nitrogen-doped carbon quantum dots were successfully prepared. These functional groups not only improve the hydrophilicity of the carbon quantum dots and the stability of the aqueous solution, but also provide action sites for metal ions.
[0067] Figure 4 This is the X-ray photoelectron spectroscopy (XPS) of nitrogen-doped carbon quantum dots N-CDs. XPS was used to further study the elemental composition of nitrogen-doped carbon quantum dots. Figure 4 As shown, three typical peaks (283.16eV, 399.47eV, 534.1eV) can be observed, belonging to C1s, N1s and O1s respectively. The element contents corresponding to the carbon quantum dots are: C1s accounts for 61.15%, N1s accounts for 9.19%, and O1s accounts for 29.65%.
[0068] Example 6
[0069] The preparation method of nitrogen-doped carbon quantum dot-modified epoxy resin is as follows:
[0070] Weigh 10 parts of epoxy resin, add 1 part of carbon quantum dots in Example 3, heat to 80° C., and react for 2 hours to obtain nano epoxy resin.
[0071] Example 7
[0072] The preparation method of nitrogen-doped carbon quantum dot-modified epoxy resin is as follows:
[0073] Weigh 20 parts of epoxy resin, add 1 part of carbon quantum dots in Example 3, heat to 80° C., and react for 2 hours to obtain nano epoxy resin.
[0074] Example 8
[0075] The preparation method of nitrogen-doped carbon quantum dot-modified epoxy resin is as follows:
[0076] Weigh 30 parts of epoxy resin, add 1 part of carbon quantum dots in Example 3, heat to 80° C., and react for 2 hours to obtain nano epoxy resin.
[0077] Example 9
[0078] The preparation method of nitrogen-doped carbon quantum dot-modified epoxy resin is as follows:
[0079] Weigh 40 parts of epoxy resin, add 1 part of carbon quantum dots in Example 3, heat to 80° C., and react for 2 hours to obtain nano epoxy resin.
[0080] Example 10
[0081] The preparation method of nitrogen-doped carbon quantum dot-modified epoxy resin is as follows:
[0082] Weigh 20 parts of epoxy resin, add 3 parts of carbon quantum dots in Example 3, heat to 100° C., and react for 3 hours to obtain nano epoxy resin.
[0083] Embodiment 11
[0084] The preparation method of nitrogen-doped carbon quantum dot-modified epoxy resin is as follows:
[0085] Weigh 20 parts of epoxy resin, add 3 parts of carbon quantum dots in Example 3, heat to 120° C., and react for 3 hours to obtain nano epoxy resin.
[0086] Example 12
[0087] The preparation method of nitrogen-doped carbon quantum dot-modified epoxy resin is as follows:
[0088] Weigh 20 parts of epoxy resin, add 3 parts of carbon quantum dots in Example 3, heat to 120° C., and react for 4 hours to obtain nano epoxy resin.
[0089] Example 13
[0090] The preparation method of nitrogen-doped carbon quantum dot-modified epoxy resin is as follows:
[0091] Weigh 20 parts of epoxy resin, add 3 parts of carbon quantum dots in Example 3, heat to 120° C., and react for 5 hours to obtain nano epoxy resin.
[0092] Embodiment 14
[0093] Taking the product in Example 11 of the present application as an example, its thermal stability was studied.
[0094] Figure 6This is the thermogravimetric diagram of epoxy resin cured with nitrogen-doped carbon quantum dots.DSC: Differential scanning calorimetry is used to determine the glass transition temperature of the cured epoxy resin. In a nitrogen atmosphere (flow rate of 60 mL / min), the temperature was raised to 250°C at a rate of 10°C / min, and the heat flow rate and temperature curve of the second temperature process were taken to analyze the data. The results show that the glass transition temperature of the cured epoxy resin is 215°C, which is much higher than the current report (Ind. Eng. Chem. Res. 2017, 56, 4938-4948; Carbon Letters 2024, 34, 477–494; Thermochimica Acta 2015, 606, 58–65)TG: A thermogravimetric analyzer was used to heat the sample from room temperature to 800°C in a nitrogen atmosphere (flow rate of 50 mL / min) at a heating rate of 10°C / min, and the mass-temperature curve was recorded. Figure 7 It can be seen that when the temperature reaches 400°C, the residual carbon rate can still reach about 90%, which further shows that the epoxy resin has thermal stability and high temperature resistance. The curing agent has obvious advantages because the carbon quantum dots, as a large conjugated system, show a large cross-linking density when curing the epoxy resin. This shows that the epoxy resin has strong hardness and high heat resistance.
[0095] It should be noted that the above content only illustrates the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications all fall within the protection scope of the claims of the present invention.
Claims
1. Application of nitrogen-doped carbon quantum dots in epoxy resin, wherein the nitrogen-doped carbon quantum dots are prepared by a method for preparing nitrogen-doped carbon quantum dots, and the method for preparing nitrogen-doped carbon quantum dots The following steps are involved: Step 1, dissolving starch and triethylenetetramine in double distilled water, and ultrasonicating for 30 minutes to obtain a mixed solution; Step 2, subjecting the mixed solution obtained in step 1 to microwave for 5 minutes, and then cooling and transferring to a polytetrafluoroethylene-lined autoclave for reaction; Step 3, cooling the yellow solution obtained by the reaction, centrifuging to remove precipitates and impurities, filtering with a 0.22 μm filter membrane, and then performing column chromatography to obtain a purified liquid; Step 4: freeze-dry the purified liquid under vacuum conditions to obtain a yellow solid powder, which is N-doped carbon quantum dots. The nitrogen-doped carbon quantum dots are configured into a 1.0 mg / mL aqueous solution and stored in a refrigerator at 4° C. for later use; In step 1, pre-weighed starch and TETA are added to double distilled water in sequence, wherein the mass ratio of starch to triethylenetetramine is 1:1 to 1:5; and the mass volume ratio of starch to double distilled water is 1:15 to 1:25; In step 2, the reaction temperature is 150-200° C. and the reaction time is 4-6 hours; In step 3, the cooling temperature is minus 60 degrees to minus 40 degrees; In step 3, the chromatography column developing agent is ethanol: water = 1:1; The particle size of the nitrogen-doped carbon quantum dots is 4.28±0.5 nm.
Citation Information
Patent Citations
A carbon quantum dot composite powder modified waterborne coating and its preparation method
CN115466552B