A Cu-loaded sulfur-doped g-C3N4 composite material and its preparation method and application

By loading amorphous Cu nanoclusters on sulfur-doped g-C3N4 nanosheets, Cu-loaded sulfur-doped g-C3N4 composite materials are solved, and the existing g-C3N4 photocatalytic antibacterial materials are achieved with high efficiency photocatalytic and antibacterial effects and reduce production costs.

CN118371259BActive Publication Date: 2024-11-19JIANGSU HENGLI CHEM FIBER
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410804641.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-11-19
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

The existing g-C3N4 photocatalytic antibacterial materials have insufficient photocatalytic properties and antibacterial properties, and the modification method is costly, so it cannot effectively improve its photocatalytic properties and antibacterial properties.

Method used

Cu-supported sulfur-doped g-C3N4 composite material is used to load amorphous Cu nanoclusters on sulfur-doped g-C3N4 nanosheets through photoreduction to form a crystalline-amorphous heterojunction structure, improving photocatalytic performance and Antibacterial properties.

Benefits of technology

The photocatalytic and antibacterial properties of the material are significantly improved, and the efficient inactivation of microorganisms such as E. coli is achieved. The preparation method is simple and low-cost, and it is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118371259B_ABST
    Figure CN118371259B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of photocatalytic antibacterial nanomaterial preparation, and discloses a Cu-loaded sulfur-doped g-C3N4 composite material and its preparation method and application. The Cu-loaded sulfur-doped g-C3N4 composite material has a crystalline-amorphous heterojunction structure, including crystalline sulfur-doped g-C3N4 nanosheets and amorphous Cu nanoclusters uniformly loaded on its surface; its preparation method is: Cu nanoclusters are loaded on sulfur-doped g-C3N4 nanosheets by a photoreduction method, that is, Cu-loaded sulfur-doped g-C3N4 composite material is obtained; the Cu-loaded sulfur-doped g-C3N4 composite material prepared by it is used as a photocatalyst to kill microorganisms. The present invention can shorten the diffusion distance of photogenerated carriers and promote the separation of photogenerated carriers through the loading of Cu elements and the synergistic effect of sulfur elements doped in the material, thereby improving the photocatalytic performance of the material, and when used for photocatalytic antibacterial materials, it has excellent antibacterial performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photocatalytic antibacterial materials, and relates to a Cu-loaded sulfur-doped gC 3 N 4 Composite material and preparation method and application thereof. Background Art

[0002] Epidemic diseases caused by harmful microorganisms such as bacteria remain an increasingly serious global health problem, and the research and development of antimicrobial agents and antimicrobial materials has become a hot topic in current research. Photocatalytic microbial inactivation technology has attracted widespread attention as a method that is broad-spectrum, efficient, safe, stable, long-lasting, heat-resistant, not prone to drug resistance, and thorough in sterilization.

[0003] Currently, gC 3 N 4 It has been widely used in photocatalytic degradation of organic pollutants, H 2 Reduction and other fields. 3 N 4 It has the unique advantages of being easy to synthesize from low-cost precursors, having a moderate bandgap (~2.7 eV), high physical and chemical stability, and both C and N being earth-abundant elements. 3 N 4 Due to the narrow visible light response range, small specific surface area, and high carrier recombination efficiency, the antibacterial performance is poor, so it is necessary to 3 N 4 Modifications were performed to improve the photocatalytic and antibacterial properties.

[0004] Existing technology for gC 3 N 4 Some attempts have been made to modify the gC. Patent document CN109526981B discloses a Ni-loaded gC 3 N 4 Preparation method of nanocomposite materials and their antibacterial properties, but the introduction of Ni does not improve gC 3 N 4 The separation of photogenerated carriers, so its photocatalytic performance and antibacterial performance cannot be greatly improved. Patent document CN115463654A discloses a Pd-Ag loaded gC 3 N 4 There is a method for preparing nanosheet photocatalysts, but it uses precious metal materials and is relatively expensive.

[0005] Patent document CN113209997A discloses a near-infrared light-responsive CuS / SC 3 N 4 Preparation method of heterojunction nanocomposite materials by hydrothermal method in SC 3 N4 CuS / SC is obtained by in-situ growth of CuS on the surface 3 N 4 The CuS loaded in the composite material is a crystalline structure. Since the crystalline material has fewer active sites than the amorphous material, the CuS / SC obtained by this method is 3 N 4 The photocatalytic performance of composite materials needs to be further improved.

[0006] As can be seen from the above, the modified gC 3 N 4 The shortcomings and deficiencies that still exist in photocatalytic antibacterial materials are: either the improvement of photocatalytic performance is limited, resulting in poor performance in degrading organic pollutants and antibacterial properties, or the cost is high.

[0007] Therefore, it is necessary to study a new type of gC with high photocatalytic performance and low cost. 3 N 4 Photocatalytic antibacterial materials are of great significance. Summary of the invention

[0008] The purpose of the present invention is to solve the problems existing in the prior art and provide a Cu-loaded sulfur-doped gC 3 N 4 Composite material and preparation method and application thereof.

[0009] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0010] A Cu-loaded sulfur-doped gC 3 N 4 Composite material with a crystalline-amorphous heterojunction structure, including crystalline sulfur-doped gC 3 N 4 Nanosheets and amorphous Cu nanoclusters uniformly loaded on their surface.

[0011] As the preferred technical solution:

[0012] A Cu-loaded sulfur-doped gC 3 N 4 Composite materials, Cu loaded sulfur-doped gC 3 N 4 The photocurrent density of the composite material is 1.8~3.2μA cm -2 .

[0013] A Cu-loaded sulfur-doped gC 3 N 4 Composite materials, sulfur-doped gC 3 N 4The diameter of the nanosheets is 100~600nm, the particle size of the Cu nanoclusters does not exceed 20nm, and the loading amount of the Cu nanoclusters is 3~50wt%.

[0014] The present invention also provides a method for preparing a Cu-loaded sulfur-doped gC 3 N 4 Composite material method, by photoreduction method on sulfur-doped gC 3 N 4 Cu nanoclusters are loaded on the nanosheets to obtain Cu-loaded sulfur-doped gC 3 N 4 Composite materials.

[0015] As the preferred technical solution:

[0016] The method described above comprises the following steps: doping gC with sulfur 3 N 4 The nanosheets were dispersed in a copper salt solution, stirred and reacted under xenon light, and post-treated (i.e., washed with deionized water and dried) to obtain Cu-loaded sulfur-doped gC 3 N 4 Composite materials.

[0017] As described above, sulfur-doped gC 3 N 4 The ratio of nanosheets to copper salt solution is 10 mg: 1-10 mL; the concentration of the copper salt solution is 1-10 M; the copper salt is one or more of copper chloride, copper sulfate, copper nitrate, basic copper carbonate and basic copper sulfate; the power of the xenon lamp is 50-1000 W; the stirring reaction time is 10-60 min, and the rate is 100-800 r / min.

[0018] As described above, sulfur-doped gC 3 N 4 The preparation process of the nanosheets is as follows: first, sulfur-doped gC is prepared by pyrolysis. 3 N 4 Micron sheet (i.e. micron-scale sheet structure), and then sulfur-doped gC 3 N 4 The micron flakes are crushed to obtain sulfur-doped gC 3 N 4 Nanosheets.

[0019] The method described above is to prepare sulfur-doped gC by thermal decomposition 3 N 4 The specific process of micron sheet is: gC 3 N 4After the precursor and the sulfur source are evenly mixed, the first pyrolysis treatment (in a muffle furnace), grinding, and the second pyrolysis treatment (in a muffle furnace) are performed in sequence to obtain sulfur-doped gC 3 N 4 Micron sheet.

[0020] As described above, gC 3 N 4 The mass ratio of precursor to sulfur source is 10:1~5; gC 3 N 4 The precursor is one or more of melamine, urea, trichloromelamine and dicyandiamide; the sulfur source is one or more of thioacetamide, thiourea, sulfur powder and sulfur-containing inorganic salt; the heating rate of the first pyrolysis treatment or the second pyrolysis treatment is 1-10°C / min, the heating end point is 450-600°C, and the holding time is 2-8h.

[0021] The method described above is to dope gC 3 N 4 The specific process of crushing the micron flakes is as follows: sulfur doped gC 3 N 4 The micron flakes are dispersed in deionized water, and the mixture is stirred to obtain a dispersion. The dispersion is treated with an ultrasonic cell crusher and then post-treated (centrifugal separation, drying). The treatment of the dispersion with an ultrasonic cell crusher is beneficial to obtain sulfur-doped gC with a smaller flake structure. 3 N 4 materials, which contributes to the exposure of their active sites.

[0022] As described above, sulfur-doped gC 3 N 4 The mass ratio of micron sheets to deionized water is 10:1~10; the power of the ultrasonic cell crusher is 500~1500W; and the processing time is 1~5h.

[0023] The present invention also provides a Cu-loaded sulfur-doped gC 3 N 4 Application of composite materials as photocatalysts to kill microorganisms.

[0024] As the preferred technical solution:

[0025] As in the applications described above, the microorganisms include Escherichia coli, Staphylococcus aureus and Candida albicans.

[0026] The specific process of the above application is as follows: Cu is loaded with sulfur-doped gC 3 N 4The composite material is dispersed in water to obtain a dispersion liquid with a concentration of 0.01-5 mg / mL, a bacterial solution containing microorganisms is added to the dispersion liquid, and the dispersion liquid is allowed to stand at 20-40° C. for 18 hours under visible light.

[0027] The Cu-loaded sulfur-doped gC 3 N 4 The composite material exhibits excellent photocatalytic performance for the following reasons:

[0028] (a) The present invention loads amorphous Cu nanoclusters on the surface of the nanosheet, and the active sites can be fully exposed. At the same time, there are usually certain defect sites in the amorphous structure, which is conducive to providing more active centers, thereby improving the catalytic performance of the material. If crystalline CuS particles are loaded on the surface of the nanosheet, the exposure of the active sites will be limited due to the large particle size;

[0029] (b) Cu-loaded sulfur-doped gC 3 N 4 Composite materials, amorphous Cu nanoclusters can be combined with crystalline sulfur-doped gC 3 N 4 A crystalline-amorphous heterojunction is formed, which has a large number of defects and can provide more electron / hole transfer channels, thereby shortening the diffusion distance of photogenerated carriers and promoting the separation of photogenerated carriers, thereby improving the photocatalytic performance of the material; if crystalline CuS particles are loaded on the surface of the nanosheet, they cannot provide corresponding electron / hole transfer channels, thereby affecting its ability to play the same role.

[0030] Beneficial effects:

[0031] (1) In the Cu-loaded sulfur-doped gC 3 N 4 In the composite material, amorphous Cu nanoclusters are uniformly loaded on sulfur-doped gC 3 N 4 The surface of the nanosheets improves the utilization rate of metal elements, and the formed crystalline-amorphous heterojunction can shorten the diffusion distance of photogenerated carriers and promote the separation of photogenerated carriers, thereby improving the photocatalytic performance of the material.

[0032] (2) The present invention first prepares sulfur-doped gC by thermal decomposition 3 N 4 Micron sheet, then sulfur doped gC 3 N 4 The micron flakes were crushed to obtain sulfur-doped gC 3 N 4 Nanosheets, which avoid gC 3 N 4The agglomeration of the active sites also helps to expose them, making them easier to contact with microorganisms such as bacteria and fungi, thereby exerting a better antibacterial effect.

[0033] (3) The Cu-loaded sulfur-doped gC provided by the present invention 3 N 4 The composite material has a significant inactivation efficiency against Escherichia coli and the like under visible light irradiation, has excellent antibacterial properties, and the preparation method is simple, low-cost, and suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The Cu-loaded sulfur-doped gC prepared in Examples 1-3 of the present invention and Comparative Example 1 3 N 4 Transmission electron microscopy images of the composite materials; in the figure, (a) is the Cu-loaded sulfur-doped gC prepared in Example 1 3 N 4 Transmission electron microscopy images of the composite materials, (b) Cu-loaded sulfur-doped gC prepared in Example 2 3 N 4 Transmission electron microscopy images of the composite materials, (c) is the Cu-loaded sulfur-doped gC prepared in Example 3 3 N 4 Transmission electron microscopy images of the composite materials, (d) is the Cu-loaded sulfur-doped gC prepared in Comparative Example 1 3 N 4 Transmission electron microscopy images of the composite material;

[0035] Figure 2 The Cu-loaded sulfur-doped gC prepared in Example 1 of the present invention 3 N 4 Element distribution diagram of composite materials; in the figure, DF4 refers to the lens used for transmission electron microscopy. The upper left is Cu loaded with sulfur-doped gC 3 N 4 Transmission electron microscopy images of the composite material. The upper right is Cu loaded with sulfur-doped gC 3 N 4 Distribution diagram of various elements in the composite material, the middle left is Cu loaded with sulfur doped gC 3 N 4 Distribution of C elements in composite materials, the middle right is Cu loaded with sulfur doped gC 3 N 4 Distribution of N elements in composite materials, the lower left is Cu loaded sulfur doped gC 3 N 4 Distribution of S elements in composite materials, the lower right is Cu loaded sulfur doped gC 3 N 4 Distribution diagram of Cu element in composite materials;

[0036] Figure 3 The Cu-loaded sulfur-doped gC prepared in Example 1 and Comparative Examples 1-3 of the present invention 3 N 4 Photocurrent density curve of the composite material;

[0037] Figure 4 The Cu-loaded sulfur-doped gC prepared in Example 1 of the present invention 3 N 4 Schematic diagram of the bactericidal performance of the composite material against Escherichia coli changing over time under the action of visible light;

[0038] Figure 5 The sulfur-doped gC without Cu loading prepared in Comparative Example 3 of the present invention 3 N 4 Schematic diagram of the time-dependent bactericidal performance of nanosheets against Escherichia coli under visible light. DETAILED DESCRIPTION

[0039] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0040] The testing methods of the relevant performance indicators in the following embodiments and comparative examples are as follows:

[0041] Photocurrent density: The photocurrent density of the sample was tested using a standard three-electrode method. The test was repeated three times and the data was recorded to obtain the average value. The counter electrode used in the test was a Pt sheet, the reference electrode was Ag / AgCl, and the working electrode was the prepared photocatalytic material (the preparation process was as follows: first, 200 μL of ethanol and 200 μL of NMP were mixed evenly, and then 5 mg of the sample was added thereto and dispersed evenly by ultrasound. While ultrasonically dispersing, 5 μL of Nafion solution (concentration of 5 wt%, CAS 31175-20-9) was added dropwise, and then evenly applied on a 1 cm × 2 cm ITO glass, and dried at 100 °C for 2 h to obtain a working electrode). The electrolyte was 0.1 mol / L NaSO 4 Solution.

[0042] Survival rate: The bacteria were cultured at 37°C until the logarithmic phase, and then centrifuged at 8000 rpm / min to collect the bacteria. Three aliquots of 1×10 7CFU / mL of bacterial solution, and finally, three 500μL dispersions (concentration of 3mg / ml, dispersed phase is sample, and dispersed medium is water) were added to the three prepared bacterial solutions (each 500μL) and plated on LB solid culture medium, then exposed to a xenon lamp (300W) equipped with an AM1.5 filter, incubated at 37°C for 18h, and finally, the bacterial concentrations in the three groups of dispersions at 2h, 4h and 6h were measured using standard plating technology, and the number of colonies in the three groups was recorded. The survival rate was calculated by the calculation formula, and the average of the three survival rates was taken. The survival rate calculation formula is: Survival rate (%) = C / C 0 ×100%, where C is the number of colonies observed after a certain period of cultivation, C 0 is the initial colony number.

[0043] Example 1

[0044] A Cu-loaded sulfur-doped gC 3 N 4 The preparation method of the composite material comprises the following steps:

[0045] (1) Preparation of raw materials;

[0046] C 3 N 4 Precursor: melamine, CAS number: 108-78-1;

[0047] Sulfur source: thiourea, CAS number: 62-56-6;

[0048] Deionized water;

[0049] Copper salt solution: the solute is copper chloride, CAS number: 10125-13-0, the solvent is deionized water, the concentration is 1M;

[0050] Ethanol;

[0051] (2) Preparation of sulfur-doped gC 3 N 4 Nanosheets;

[0052] (2.1) The mass ratio of gC is 10:1. 3 N 4 The precursor and the sulfur source were ground in a mortar for 20 minutes and mixed evenly, then placed in a porcelain boat, heated to 500°C in a muffle furnace at a heating rate of 2°C / min and kept warm for 8 hours, and then ground again. After grinding, the temperature was raised to 450°C in a muffle furnace at a heating rate of 1°C / min and kept warm for 5 hours to obtain sulfur-doped gC 3 N 4 Micron sheet;

[0053] (2.2) The sulfur-doped gC 3 N 4 The micronized flakes were dispersed in deionized water and stirred thoroughly to obtain dispersion I. The dispersion I was treated with an ultrasonic cell crusher with a power of 500 W for 3 h, and then post-treated (centrifugal separation, drying) to obtain sulfur-doped gC 3 N 4 Nanosheets; wherein sulfur-doped gC 3 N 4 The mass ratio of micron sheets to deionized water is 10:1;

[0054] Sulfur-doped gC 3 N 4 The diameter of the nanosheets is 400-600nm;

[0055] (3) The sulfur-doped gC prepared in step (2) 3 N 4 The nanosheets were dispersed in the copper salt solution and stirred for 30 min. Then, they were stirred at a rate of 200 r / min for 10 min under the irradiation of a 300 W xenon lamp. Then, they were washed three times by centrifugation with deionized water and ethanol respectively, and then dried in a vacuum oven at 60 ° C for 12 h to obtain Cu-loaded sulfur-doped gC 3 N 4 Composite material; wherein sulfur-doped gC 3 N 4 The ratio of nanosheets to copper salt solution was 10 mg:1 mL.

[0056] The final Cu-loaded sulfur-doped gC 3 N 4 Composite material (transmission electron microscope image as shown Figure 1 As shown in (a), the distribution diagram of each element is as follows Figure 2 As shown in Figure 2, it has a crystalline-amorphous heterojunction structure, which is composed of crystalline sulfur-doped gC 3 N 4 The nanosheets are composed of amorphous Cu nanoclusters uniformly loaded on the surface. The particle size of the Cu nanoclusters is 2-5nm, and the loading amount of the Cu nanoclusters is 3wt%. 3 N 4 The photocurrent density of the composite material is 2.2 μA cm -2 ,from Figure 3 It can be seen that gC 3 N 4 After sulfur doping and Cu nanoclusters loading, the photocurrent density has been significantly improved. This is because gC 3 N 4The synergistic effect with sulfur and copper shortens the diffusion distance of photogenerated carriers and promotes the separation of photogenerated carriers; the photocurrent of materials not treated with ultrasonic cell crusher is slightly smaller than that of treated materials due to limited exposure of active sites.

[0057] Cu-loaded sulfur-doped gC 3 N 4 Application of composite materials: the Cu prepared above is loaded with sulfur-doped gC 3 N 4 The composite material was dispersed in water to obtain a dispersion II with a concentration of 3 mg / mL. The bacterial solution (containing 10 7 CFU / mL Escherichia coli), the volume ratio of dispersion II to bacterial solution was 1:1, and the cells were incubated at 37°C under visible light for 18 h.

[0058] Through the above tests, we can know that Figure 4 As shown in the figure, after the dispersion II was left to stand for 6 hours after the bacterial solution was added, the survival rate of Escherichia coli was 0%, and the Escherichia coli was completely killed. Therefore, the Cu-loaded sulfur-doped gC prepared above 3 N 4 The composite material has significant photocatalytic bactericidal properties.

[0059] Comparative Example 1

[0060] A Cu-loaded sulfur-doped gC 3 N 4 The preparation method of the composite material is basically the same as that of Example 1, except that step (2.2) is not performed, and the sulfur-doped gC in step (3) is 3 N 4 The nanosheets were replaced with the sulfur-doped gC prepared in step (2.1). 3 N 4 Micron sheet.

[0061] The final Cu-loaded sulfur-doped gC 3 N 4 The photocurrent density of the composite material is 1.4 μA cm -2 (The photocurrent density is Figure 3 The transmission electron microscope image is shown in Figure 1 As shown in (d), it can be seen from the figure that Cu loaded sulfur doped gC 3 N 4 The composite material consists of large platelet structures with platelet size >1 μm.

[0062] Cu-loaded sulfur-doped gC 3 N 4 The application of the composite material is basically the same as in Example 1, except that the Cu used is loaded with sulfur-doped gC3 N 4 The composite material is prepared in this comparative example.

[0063] The above test shows that after the dispersion II with the bacterial solution added was left to stand for 6 hours, the survival rate of E. coli was 15%, and the E. coli was not completely killed.

[0064] Comparing Comparative Example 1 with Example 1, it can be seen that the Cu loaded with sulfur-doped gC prepared in Comparative Example 1 3 N 4 The bactericidal performance of the composite material is poor, which is because the comparative example 1 does not dope gC with sulfur. 3 N 4 The micron sheet is subjected to ultrasonic cell pulverization treatment, which will cause sulfur-doped gC 3 N 4 The nano-scaling of micron sheets helps to expose their active sites, thereby forming more crystalline-amorphous heterojunction structures in the subsequent Cu loading process, which is beneficial to improving the photocatalytic performance of the material.

[0065] Comparative Example 2

[0066] A Cu-loaded gC 3 N 4 The preparation method of the composite material is basically the same as that of Example 1, except that no sulfur source is added in step (2).

[0067] The final Cu-loaded gC 3 N 4 The photocurrent density of the composite material is 0.8 μA cm -2 (The photocurrent density is Figure 3 as shown).

[0068] Cu loading gC 3 N 4 The application of the composite material is basically the same as in Example 1, except that the Cu loading gC 3 N 4 The composite material is prepared in this comparative example.

[0069] The above test shows that after the dispersion II with the bacterial solution added was left to stand for 6 hours, the survival rate of E. coli was 8%, and the E. coli was not completely killed.

[0070] Comparing Comparative Example 2 with Example 1, it can be seen that the Cu-loaded gC 3 N 4 The bactericidal performance of the composite material is poor, which is because the comparative example 2 does not 3 N 4 The nanosheets are doped with sulfur. On the one hand, sulfur doping will make gC 3 N4 The nanosheets form a porous structure to expose more active sites, which can enhance the gC 3 N 4 The absorption capacity of visible light, while the gC prepared in Comparative Example 2 3 N 4 Due to the lack of sulfur doping, the active sites of the nanosheets are not sufficiently exposed, and the formed crystalline-amorphous heterojunction structure is less, resulting in the Cu loading of gC 3 N 4 There are fewer electron / hole transfer channels, which cannot shorten the diffusion distance of photogenerated carriers and promote the separation of photogenerated carriers, making Cu loaded with gC 3 N 4 The composite material has poor photocatalytic performance, which affects its bactericidal performance.

[0071] Comparative Example 3

[0072] A sulfur-doped gC 3 N 4 The preparation method of the nanosheets is the same as step (2) of Example 1.

[0073] The final sulfur-doped gC 3 N 4 The photocurrent density of the nanosheet is 0.4 μA cm -2 (The photocurrent density is Figure 3 as shown).

[0074] Sulfur-doped gC 3 N 4 Application of nanosheets, the sulfur-doped gC 3 N 4 The nanosheets were dispersed in water to obtain dispersion II (with the same concentration as in Example 1), bacterial solution (with the same ingredients and addition amount as in Example 1) was added to the dispersion II, and the dispersion was allowed to stand under visible light (with the same standing conditions as in Example 1).

[0075] Through the above tests, we can know that Figure 5 As shown, after the dispersion II with the bacterial solution was left to stand for 6 hours, the survival rate of E. coli was 10%, and some E. coli were still not killed.

[0076] Comparing Comparative Example 3 with Example 1, it can be seen that the sulfur-doped gC prepared in Comparative Example 3 3 N 4 The antibacterial performance and photocurrent density of the nanosheets are greatly reduced. This is because although sulfur-doped gC 3 N 4 It is also a good antibacterial material, but its antibacterial performance is far inferior to that of many metal elements. The amorphous Cu nanoclusters and crystalline sulfur-doped gC 3N 4 The combination can form a crystalline-amorphous heterojunction structure. The crystalline-amorphous heterojunction has a large number of defects, which can provide more electron / hole transfer channels, thereby shortening the diffusion distance of photogenerated carriers and promoting the separation of photogenerated carriers, thereby improving the photocatalytic performance of the material.

[0077] Example 2

[0078] A Cu-loaded sulfur-doped gC 3 N 4 The preparation method of the composite material comprises the following steps:

[0079] (1) Preparation of raw materials;

[0080] C 3 N 4 Precursor: melamine, CAS number: 108-78-1;

[0081] Sulfur source: thiourea, CAS number: 62-56-6;

[0082] Deionized water;

[0083] Copper salt solution: the solute is copper chloride, CAS number: 10125-13-0, the solvent is deionized water, the concentration is 2M;

[0084] Ethanol;

[0085] (2) Preparation of sulfur-doped gC 3 N 4 Nanosheets;

[0086] (2.1) The mass ratio of gC is 10:2. 3 N 4 The precursor and the sulfur source were ground in a mortar for 30 minutes and mixed evenly, then placed in a porcelain boat, heated to 550°C in a muffle furnace at a heating rate of 3°C / min and kept warm for 5 hours, and then ground again. After grinding, the temperature was raised to 500°C in a muffle furnace at a heating rate of 2°C / min and kept warm for 4 hours to obtain sulfur-doped gC 3 N 4 Micron sheet;

[0087] (2.2) The sulfur-doped gC 3 N 4 The micronized flakes were dispersed in deionized water and stirred thoroughly to obtain dispersion I. The dispersion I was treated with an ultrasonic cell crusher with a power of 800 W for 2 h, and then post-treated (centrifugal separation, drying) to obtain sulfur-doped gC 3 N 4 Nanosheets; wherein sulfur-doped gC 3 N 4The mass ratio of micron sheets to deionized water is 10:2;

[0088] Sulfur-doped gC 3 N 4 The diameter of the nanosheets is 200-350 nm;

[0089] (3) The sulfur-doped gC prepared in step (2) 3 N 4 The nanosheets were dispersed in the copper salt solution and stirred for 30 min. Then, they were stirred at 300 r / min for 10 min under the irradiation of a 200 W xenon lamp. Then, they were washed three times by centrifugation with deionized water and ethanol respectively, and then dried in a vacuum oven at 60 ° C for 12 h to obtain Cu-loaded sulfur-doped gC 3 N 4 Composite material; wherein sulfur-doped gC 3 N 4 The ratio of nanosheets to copper salt solution was 10 mg:2 mL.

[0090] The final Cu-loaded sulfur-doped gC 3 N 4 Composite material (transmission electron microscope image as shown Figure 1 (b) has a crystalline-amorphous heterojunction structure, which is composed of crystalline sulfur-doped gC 3 N 4 The nanosheets are composed of amorphous Cu nanoclusters uniformly loaded on the surface. The particle size of the Cu nanoclusters is 5-8nm, and the loading amount of the Cu nanoclusters is 12wt%. 3 N 4 The photocurrent density of the composite material is 1.8 μA cm -2 .

[0091] Cu-loaded sulfur-doped gC 3 N 4 Application of composite materials: the Cu prepared above is loaded with sulfur-doped gC 3 N 4 The composite material was dispersed in water to obtain a dispersion II with a concentration of 1 mg / mL. The bacterial solution (containing 10 6 CFU / mL Escherichia coli), the volume ratio of dispersion II to bacterial solution was 1:2, and the samples were incubated at 35°C under visible light for 18 h.

[0092] The above test shows that after the dispersion II with the bacterial solution was left to stand for 6 hours, the survival rate of E. coli was 0%, and the E. coli was completely killed. Therefore, the Cu-loaded sulfur-doped gC prepared above 3 N 4 The composite material has significant photocatalytic bactericidal properties.

[0093] Example 3

[0094] A Cu-loaded sulfur-doped gC 3 N 4 The preparation method of the composite material comprises the following steps:

[0095] (1) Preparation of raw materials;

[0096] C 3 N 4 Precursor: melamine, CAS number: 108-78-1;

[0097] Sulfur source: thioacetamide, CAS number: 62-55-5;

[0098] Deionized water;

[0099] Copper salt solution: the solute is copper sulfate, CAS number: 7758-99-8, the solvent is deionized water, the concentration is 1M;

[0100] Ethanol;

[0101] (2) Preparation of sulfur-doped gC 3 N 4 Nanosheets;

[0102] (2.1) The mass ratio of gC is 10:3. 3 N 4 The precursor and the sulfur source were ground in a mortar for 20 minutes and mixed evenly, then placed in a porcelain boat, heated to 580°C in a muffle furnace at a heating rate of 4°C / min and kept warm for 4 hours, and then ground again. After grinding, the temperature was raised to 550°C in a muffle furnace at a heating rate of 5°C / min and kept warm for 2 hours to obtain sulfur-doped gC 3 N 4 Micron sheet;

[0103] (2.2) The sulfur-doped gC 3 N 4 The micronized flakes were dispersed in deionized water and stirred thoroughly to obtain dispersion I. The dispersion I was treated with an ultrasonic cell crusher with a power of 1000 W for 1 h, and then post-treated (centrifugal separation, drying) to obtain sulfur-doped gC 3 N 4 Nanosheets; wherein sulfur-doped gC 3 N 4 The mass ratio of micron sheets to deionized water is 10:4;

[0104] Sulfur-doped gC 3 N 4 The diameter of the nanosheets is 150-250 nm;

[0105] (3) The sulfur-doped gC prepared in step (2) 3 N 4 The nanosheets were dispersed in the copper salt solution and stirred for 30 min. Then, they were stirred at 300 r / min for 30 min under the irradiation of a 1000 W xenon lamp. Then, they were washed three times by centrifugation with deionized water and ethanol respectively, and then dried in a vacuum oven at 60 ° C for 12 h to obtain Cu-loaded sulfur-doped gC 3 N 4 Composite material; wherein sulfur-doped gC 3 N 4 The ratio of nanosheets to copper salt solution was 10 mg:3 mL.

[0106] The final Cu-loaded sulfur-doped gC 3 N 4 Composite material (transmission electron microscope image as shown Figure 1 (c) has a crystalline-amorphous heterojunction structure, which is composed of crystalline sulfur-doped gC 3 N 4 The nanosheets are composed of amorphous Cu nanoclusters uniformly loaded on the surface. The particle size of the Cu nanoclusters is 3-6nm, and the loading amount of the Cu nanoclusters is 8wt%. 3 N 4 The photocurrent density of the composite material is 2.1 μA cm -2 .

[0107] Cu-loaded sulfur-doped gC 3 N 4 Application of composite materials: the Cu prepared above is loaded with sulfur-doped gC 3 N 4 The composite material was dispersed in water to obtain a dispersion II with a concentration of 2 mg / mL. The bacterial solution (containing 10 6 CFU / mL Escherichia coli), the volume ratio of dispersion II to bacterial solution was 1:5, and the samples were allowed to stand at 20°C under visible light for 18 h.

[0108] The above test shows that after the dispersion II with the bacterial solution was left to stand for 6 hours, the survival rate of E. coli was 0%, and the E. coli was completely killed. Therefore, the Cu-loaded sulfur-doped gC prepared above 3 N 4 The composite material has significant photocatalytic bactericidal properties.

[0109] Example 4

[0110] A Cu-loaded sulfur-doped gC 3 N 4The preparation method of the composite material comprises the following steps:

[0111] (1) Preparation of raw materials;

[0112] C 3 N 4 Precursor: urea, CAS number: 57-13-6;

[0113] Sulfur source: thioacetamide, CAS number: 62-55-5;

[0114] Deionized water;

[0115] Copper salt solution: the solute is copper sulfate, CAS number: 7758-99-8, the solvent is deionized water, the concentration is 10M;

[0116] Ethanol;

[0117] (2) Preparation of sulfur-doped gC 3 N 4 Nanosheets;

[0118] (2.1) The mass ratio of gC is 10:5. 3 N 4 The precursor and the sulfur source were ground in a mortar for 20 minutes and mixed evenly, then placed in a porcelain boat, heated to 580°C in a muffle furnace at a heating rate of 3°C / min and kept warm for 3 hours, and then ground again. After grinding, the temperature was raised to 550°C in a muffle furnace at a heating rate of 10°C / min and kept warm for 5 hours to obtain sulfur-doped gC 3 N 4 Micron sheet;

[0119] (2.2) The sulfur-doped gC 3 N 4 The micronized flakes were dispersed in deionized water and stirred thoroughly to obtain dispersion I. The dispersion I was treated with an ultrasonic cell crusher with a power of 900 W for 4 h, and then post-treated (centrifugal separation, drying) to obtain sulfur-doped gC 3 N 4 Nanosheets; wherein sulfur-doped gC 3 N 4 The mass ratio of micron sheets to deionized water is 10:5;

[0120] Sulfur-doped gC 3 N 4 The diameter of the nanosheets is 100-200 nm;

[0121] (3) The sulfur-doped gC prepared in step (2) 3 N 4The nanosheets were dispersed in the copper salt solution and stirred for 30 min. Then, they were stirred at a rate of 500 r / min for 30 min under the irradiation of a 400 W xenon lamp. Then, they were washed three times by centrifugation with deionized water and ethanol respectively, and then dried in a vacuum oven at 60 ° C for 12 h to obtain Cu-loaded sulfur-doped gC 3 N 4 Composite material; wherein sulfur-doped gC 3 N 4 The ratio of nanosheets to copper salt solution was 10 mg:5 mL.

[0122] The final Cu-loaded sulfur-doped gC 3 N 4 The composite material has a crystalline-amorphous heterojunction structure, which is composed of crystalline sulfur-doped gC 3 N 4 The nanosheets are composed of amorphous Cu nanoclusters uniformly loaded on the surface. The particle size of the Cu nanoclusters is 15-18nm, and the loading amount of the Cu nanoclusters is 40wt%. 3 N 4 The photocurrent density of the composite material is 2.9 μA cm -2 .

[0123] Cu-loaded sulfur-doped gC 3 N 4 Application of composite materials: the Cu prepared above is loaded with sulfur-doped gC 3 N 4 The composite material was dispersed in water to obtain a dispersion II with a concentration of 2 mg / mL. The bacterial solution (containing 10 8 CFU / mL Escherichia coli), the volume ratio of dispersion II to bacterial solution was 1:0.1, and the samples were allowed to stand at 25°C under visible light for 18 h.

[0124] The above test shows that after the dispersion II with the bacterial solution was left to stand for 6 hours, the survival rate of E. coli was 0%, and the E. coli was completely killed. Therefore, the Cu-loaded sulfur-doped gC prepared above 3 N 4 The composite material has significant photocatalytic bactericidal properties.

[0125] Example 5

[0126] A Cu-loaded sulfur-doped gC 3 N 4 The preparation method of the composite material comprises the following steps:

[0127] (1) Preparation of raw materials;

[0128] C 3 N 4Precursor: trichloromelamine, CAS No.: 7673-09-8;

[0129] Sulfur source: sulfur powder, CAS number: 7704-34-9;

[0130] Deionized water;

[0131] Copper salt solution: the solute is copper nitrate, CAS number: 10031-43-3, the solvent is deionized water, the concentration is 5M;

[0132] Ethanol;

[0133] (2) Preparation of sulfur-doped gC 3 N 4 Nanosheets;

[0134] (2.1) The mass ratio of gC is 10:2. 3 N 4 The precursor and the sulfur source were ground in a mortar for 20 minutes and mixed evenly, then placed in a porcelain boat, heated to 600°C in a muffle furnace at a heating rate of 5°C / min and kept warm for 2 hours, and then ground again. After grinding, the temperature was raised to 550°C in a muffle furnace at a heating rate of 8°C / min and kept warm for 2 hours to obtain sulfur-doped gC 3 N 4 Micron sheet;

[0135] (2.2) The sulfur-doped gC 3 N 4 The micronized flakes were dispersed in deionized water and stirred thoroughly to obtain dispersion I. The dispersion I was treated with an ultrasonic cell crusher with a power of 1000 W for 5 h, and then post-treated (centrifugal separation, drying) to obtain sulfur-doped gC 3 N 4 Nanosheets; wherein sulfur-doped gC 3 N 4 The mass ratio of micron sheets to deionized water is 10:8;

[0136] Sulfur-doped gC 3 N 4 The diameter of the nanosheets is 100-150 nm;

[0137] (3) The sulfur-doped gC prepared in step (2) 3 N 4 The nanosheets were dispersed in the copper salt solution and stirred for 30 min. Then, they were stirred at 600 r / min for 20 min under 50 W xenon lamp illumination. Then, they were washed three times by centrifugation with deionized water and ethanol respectively, and then dried in a vacuum oven at 60 °C for 12 h to obtain Cu-loaded sulfur-doped gC. 3 N 4Composite material; wherein sulfur-doped gC 3 N 4 The ratio of nanosheets to copper salt solution was 10 mg:8 mL.

[0138] The final Cu-loaded sulfur-doped gC 3 N 4 The composite material has a crystalline-amorphous heterojunction structure, which is composed of crystalline sulfur-doped gC 3 N 4 The nanosheets are composed of amorphous Cu nanoclusters uniformly loaded on the surface. The particle size of the Cu nanoclusters is 12-16nm, and the loading amount of the Cu nanoclusters is 37wt%. 3 N 4 The photocurrent density of the composite material is 1.9 μA cm -2 .

[0139] Cu-loaded sulfur-doped gC 3 N 4 Application of composite materials: the Cu prepared above is loaded with sulfur-doped gC 3 N 4 The composite material was dispersed in water to obtain a dispersion II with a concentration of 0.01 mg / mL. The bacterial solution (containing 10 7 CFU / mL Escherichia coli), the volume ratio of dispersion II to bacterial solution was 1:8, and the samples were allowed to stand at 40°C under visible light for 18 h.

[0140] The above test shows that after the dispersion II with the bacterial solution was left to stand for 6 hours, the survival rate of E. coli was 0%, and the E. coli was completely killed. Therefore, the Cu-loaded sulfur-doped gC prepared above 3 N 4 The composite material has significant photocatalytic bactericidal properties.

[0141] Example 6

[0142] A Cu-loaded sulfur-doped gC 3 N 4 The preparation method of the composite material comprises the following steps:

[0143] (1) Preparation of raw materials;

[0144] C 3 N 4 Precursor: dicyandiamide, CAS No.: 461-58-5;

[0145] Sulfur source: sulfur powder, CAS number: 7704-34-9;

[0146] Deionized water;

[0147] Copper salt solution: the solute is basic copper carbonate, CAS number: 166733-69-3, the solvent is deionized water, the concentration is 3M;

[0148] Ethanol;

[0149] (2) Preparation of sulfur-doped gC 3 N 4 Nanosheets;

[0150] (2.1) The mass ratio of gC is 10:1. 3 N 4 The precursor and the sulfur source were ground in a mortar for 20 minutes and mixed evenly, then placed in a porcelain boat, heated to 550°C in a muffle furnace at a heating rate of 5°C / min and kept warm for 5 hours, and then ground again. After grinding, the temperature was raised to 500°C in a muffle furnace at a heating rate of 6°C / min and kept warm for 6 hours to obtain sulfur-doped gC 3 N 4 Micron sheet;

[0151] (2.2) The sulfur-doped gC 3 N 4 The micronized flakes were dispersed in deionized water and stirred thoroughly to obtain dispersion I. The dispersion I was treated with an ultrasonic cell crusher with a power of 1100 W for 2 h, and then post-treated (centrifugal separation, drying) to obtain sulfur-doped gC 3 N 4 Nanosheets; wherein sulfur-doped gC 3 N 4 The mass ratio of micron sheets to deionized water is 10:9;

[0152] Sulfur-doped gC 3 N 4 The diameter of the nanosheets is 150-250 nm;

[0153] (3) The sulfur-doped gC prepared in step (2) 3 N 4 The nanosheets were dispersed in the copper salt solution and stirred for 30 min. After stirring at 700 r / min for 50 min under 200 W xenon lamp irradiation, they were washed three times by centrifugation with deionized water and ethanol respectively, and then dried in a vacuum oven at 60 ° C for 12 h to obtain Cu-loaded sulfur-doped gC 3 N 4 Composite material; wherein sulfur-doped gC 3 N 4 The ratio of nanosheets to copper salt solution was 10 mg:9 mL.

[0154] The final Cu-loaded sulfur-doped gC 3 N 4The composite material has a crystalline-amorphous heterojunction structure, which is composed of crystalline sulfur-doped gC 3 N 4 The nanosheets are composed of amorphous Cu nanoclusters uniformly loaded on the surface. The particle size of the Cu nanoclusters is 10-13nm, and the loading amount of the Cu nanoclusters is 22wt%. 3 N 4 The photocurrent density of the composite material is 2.4 μA cm -2 .

[0155] Cu-loaded sulfur-doped gC 3 N 4 Application of composite materials: the Cu prepared above is loaded with sulfur-doped gC 3 N 4 The composite material was dispersed in water to obtain a dispersion II with a concentration of 4 mg / mL. The bacterial solution (containing 10 6 CFU / mL Escherichia coli), the volume ratio of dispersion II to bacterial solution was 1:10, and the cells were incubated at 32°C under visible light for 18 h.

[0156] The above test shows that after the dispersion II with the bacterial solution was left to stand for 6 hours, the survival rate of E. coli was 0%, and the E. coli was completely killed. Therefore, the Cu-loaded sulfur-doped gC prepared above 3 N 4 The composite material has significant photocatalytic bactericidal properties.

[0157] Example 7

[0158] A Cu-loaded sulfur-doped gC 3 N 4 The preparation method of the composite material comprises the following steps:

[0159] (1) Preparation of raw materials;

[0160] C 3 N 4 Precursor: dicyandiamide, CAS No.: 461-58-5;

[0161] Sulfur source: thioacetamide, CAS number: 62-55-5;

[0162] Deionized water;

[0163] Copper salt solution: the solute is basic copper carbonate, CAS number: 166733-69-3, the solvent is deionized water, the concentration is 2M;

[0164] Ethanol;

[0165] (2) Preparation of sulfur-doped gC 3 N4 Nanosheets;

[0166] (2.1) The mass ratio of gC is 10:5. 3 N 4 The precursor and the sulfur source were ground in a mortar for 20 minutes and mixed evenly, then placed in a porcelain boat, heated to 600°C in a muffle furnace at a heating rate of 4°C / min and kept warm for 2 hours, and then ground again. After grinding, the temperature was raised to 560°C in a muffle furnace at a heating rate of 2°C / min and kept warm for 3 hours to obtain sulfur-doped gC 3 N 4 Micron sheet;

[0167] (2.2) The sulfur-doped gC 3 N 4 The micronized flakes were dispersed in deionized water and stirred thoroughly to obtain dispersion I. The dispersion I was treated with an ultrasonic cell crusher with a power of 1200 W for 1 h, and then post-treated (centrifugal separation, drying) to obtain sulfur-doped gC 3 N 4 Nanosheets; wherein sulfur-doped gC 3 N 4 The mass ratio of micron sheets to deionized water is 10:10;

[0168] Sulfur-doped gC 3 N 4 The diameter of the nanosheets is 200-300 nm;

[0169] (3) The sulfur-doped gC prepared in step (2) 3 N 4 The nanosheets were dispersed in the copper salt solution and stirred for 30 min. Then, they were stirred at a rate of 500 r / min for 60 min under the irradiation of a 300 W xenon lamp. Then, they were washed three times by centrifugation with deionized water and ethanol respectively, and then dried in a vacuum oven at 60 ° C for 12 h to obtain Cu-loaded sulfur-doped gC 3 N 4 Composite material; wherein sulfur-doped gC 3 N 4 The ratio of nanosheets to copper salt solution was 10 mg:10 mL.

[0170] The final Cu-loaded sulfur-doped gC 3 N 4 The composite material has a crystalline-amorphous heterojunction structure, which is composed of crystalline sulfur-doped gC 3 N 4 The nanosheets are composed of amorphous Cu nanoclusters uniformly loaded on the surface. The particle size of the Cu nanoclusters is 7-10nm, and the loading amount of the Cu nanoclusters is 19wt%.3 N 4 The photocurrent density of the composite material is 2.2 μA cm -2 .

[0171] Cu-loaded sulfur-doped gC 3 N 4 Application of composite materials: the Cu prepared above is loaded with sulfur-doped gC 3 N 4 The composite material was dispersed in water to obtain a dispersion II with a concentration of 3 mg / mL. The bacterial solution (containing 10 6 CFU / mL Escherichia coli), the volume ratio of dispersion II to bacterial solution was 1:0.5, and the samples were allowed to stand at 24°C under visible light for 18 h.

[0172] The above test shows that after the dispersion II with the bacterial solution was left to stand for 6 hours, the survival rate of E. coli was 0%, and the E. coli was completely killed. Therefore, the Cu-loaded sulfur-doped gC prepared above 3 N 4 The composite material has significant photocatalytic bactericidal properties.

[0173] Example 8

[0174] A Cu-loaded sulfur-doped gC 3 N 4 The preparation method of the composite material comprises the following steps:

[0175] (1) Preparation of raw materials;

[0176] C 3 N 4 Precursor: trichloromelamine, CAS No.: 7673-09-8;

[0177] Sulfur source: thiourea, CAS number: 62-56-6;

[0178] Deionized water;

[0179] Copper salt solution: the solute is basic copper sulfate, CAS number: 1344-73-6, the solvent is deionized water, the concentration is 8M;

[0180] Ethanol;

[0181] (2) Preparation of sulfur-doped gC 3 N 4 Nanosheets;

[0182] (2.1) The mass ratio of gC is 10:3. 3 N 4The precursor and the sulfur source were ground in a mortar for 20 minutes and mixed evenly, then placed in a porcelain boat, heated to 580°C in a muffle furnace at a heating rate of 5°C / min and kept warm for 3 hours, and then ground again. After grinding, the temperature was raised to 550°C in a muffle furnace at a heating rate of 3°C / min and kept warm for 2 hours to obtain sulfur-doped gC 3 N 4 Micron sheet;

[0183] (2.2) The sulfur-doped gC 3 N 4 The micronized flakes were dispersed in deionized water and stirred thoroughly to obtain dispersion I. The dispersion I was treated with an ultrasonic cell crusher with a power of 1500 W for 1 h, and then post-treated (centrifugal separation, drying) to obtain sulfur-doped gC 3 N 4 Nanosheets; wherein sulfur-doped gC 3 N 4 The mass ratio of micron sheets to deionized water is 10:10;

[0184] Sulfur-doped gC 3 N 4 The diameter of the nanosheets is 200-250 nm;

[0185] (3) The sulfur-doped gC prepared in step (2) 3 N 4 The nanosheets were dispersed in the copper salt solution and stirred for 30 min. Then, they were stirred at 800 r / min for 10 min under 800 W xenon lamp irradiation. Then, they were washed three times by centrifugation with deionized water and ethanol respectively, and then dried in a vacuum oven at 60 °C for 12 h to obtain Cu-loaded sulfur-doped gC. 3 N 4 Composite material; wherein sulfur-doped gC 3 N 4 The ratio of nanosheets to copper salt solution was 10 mg:10 mL.

[0186] The final Cu-loaded sulfur-doped gC 3 N 4 The composite material has a crystalline-amorphous heterojunction structure, which is composed of crystalline sulfur-doped gC 3 N 4 The nanosheets are composed of amorphous Cu nanoclusters uniformly loaded on the surface. The particle size of the Cu nanoclusters is 15-19nm, and the loading amount of the Cu nanoclusters is 50wt%; Cu loaded sulfur-doped gC 3 N 4 The photocurrent density of the composite material is 3.2 μA cm -2 .

[0187] Cu-loaded sulfur-doped gC 3 N 4 Application of composite materials: the Cu prepared above is loaded with sulfur-doped gC 3 N 4 The composite material was dispersed in water to obtain a dispersion II with a concentration of 5 mg / mL. The bacterial solution (containing 10 8 CFU / mL Escherichia coli), the volume ratio of dispersion II to bacterial solution was 1:6, and the cells were incubated at 38°C under visible light for 18 h.

[0188] The above test shows that after the dispersion II with the bacterial solution was left to stand for 6 hours, the survival rate of E. coli was 0%, and the E. coli was completely killed. Therefore, the Cu-loaded sulfur-doped gC prepared above 3 N 4 The composite material has significant photocatalytic bactericidal properties.

[0189] Example 9

[0190] A Cu-loaded sulfur-doped gC 3 N 4 The preparation method of the composite material comprises the following steps:

[0191] (1) Preparation of raw materials;

[0192] C 3 N 4 Precursor: urea, CAS number: 57-13-6;

[0193] Sulfur source: thiourea, CAS number: 62-56-6;

[0194] Deionized water;

[0195] Copper salt solution: the solute is basic copper sulfate, CAS number: 1344-73-6, the solvent is deionized water, the concentration is 2M;

[0196] Ethanol;

[0197] (2) Preparation of sulfur-doped gC 3 N 4 Nanosheets;

[0198] (2.1) The mass ratio of gC is 10:2. 3 N 4 The precursor and the sulfur source were ground in a mortar for 20 minutes and mixed evenly, then placed in a porcelain boat, heated to 600°C in a muffle furnace at a heating rate of 10°C / min and kept warm for 3 hours, and then ground again. After grinding, the temperature was raised to 580°C in a muffle furnace at a heating rate of 4°C / min and kept warm for 2 hours to obtain sulfur-doped gC 3 N 4Micron sheet;

[0199] (2.2) The sulfur-doped gC 3 N 4 The micronized flakes were dispersed in deionized water and stirred thoroughly to obtain dispersion I. The dispersion I was treated with an ultrasonic cell crusher with a power of 1200 W for 3 h, and then post-treated (centrifugal separation, drying) to obtain sulfur-doped gC 3 N 4 Nanosheets; wherein sulfur-doped gC 3 N 4 The mass ratio of micron sheets to deionized water is 10:4;

[0200] Sulfur-doped gC 3 N 4 The diameter of the nanosheets is 100-200 nm;

[0201] (3) The sulfur-doped gC prepared in step (2) 3 N 4 The nanosheets were dispersed in the copper salt solution and stirred for 30 min. Then, they were stirred at 600 r / min for 20 min under the irradiation of a 600 W xenon lamp. Then, they were washed three times by centrifugation with deionized water and ethanol respectively, and then dried in a vacuum oven at 60 ° C for 12 h to obtain Cu-loaded sulfur-doped gC 3 N 4 Composite material; wherein sulfur-doped gC 3 N 4 The ratio of nanosheets to copper salt solution was 10 mg:4 mL.

[0202] The final Cu-loaded sulfur-doped gC 3 N 4 The composite material has a crystalline-amorphous heterojunction structure, which is composed of crystalline sulfur-doped gC 3 N 4 The nanosheets are composed of amorphous Cu nanoclusters uniformly loaded on the surface. The particle size of the Cu nanoclusters is 2-5nm, and the loading amount of the Cu nanoclusters is 10wt%. 3 N 4 The photocurrent density of the composite material is 2.3 μA cm -2 .

[0203] Cu-loaded sulfur-doped gC 3 N 4 Application of composite materials: the Cu prepared above is loaded with sulfur-doped gC 3 N 4 The composite material was dispersed in water to obtain a dispersion II with a concentration of 0.01 mg / mL. The bacterial solution (containing 107 CFU / mL Escherichia coli), the volume ratio of dispersion II to bacterial solution was 1:3, and the samples were allowed to stand at 30°C under visible light for 18 h.

[0204] The above test shows that after the dispersion II with the bacterial solution was left to stand for 6 hours, the survival rate of E. coli was 0%, and the E. coli was completely killed. Therefore, the Cu-loaded sulfur-doped gC prepared above 3 N 4 The composite material has significant photocatalytic bactericidal properties.

[0205] Example 10

[0206] A Cu-loaded sulfur-doped gC 3 N 4 The preparation method of the composite material comprises the following steps:

[0207] (1) Preparation of raw materials;

[0208] C 3 N 4 Precursor: urea, CAS number: 57-13-6;

[0209] Sulfur source: sulfur powder, CAS number: 7704-34-9;

[0210] Deionized water;

[0211] Copper salt solution: the solute is copper chloride, CAS number: 10125-13-0, the solvent is deionized water, the concentration is 8M;

[0212] Ethanol;

[0213] (2) Preparation of sulfur-doped gC 3 N 4 Nanosheets;

[0214] (2.1) The mass ratio of gC is 10:1. 3 N 4 The precursor and the sulfur source were ground in a mortar for 20 minutes and mixed evenly, then placed in a porcelain boat, heated to 560°C in a muffle furnace at a heating rate of 8°C / min and kept warm for 8 hours, and then ground again. After grinding, the temperature was raised to 520°C in a muffle furnace at a heating rate of 1°C / min and kept warm for 3 hours to obtain sulfur-doped gC 3 N 4 Micron sheet;

[0215] (2.2) The sulfur-doped gC 3 N 4The micronized flakes were dispersed in deionized water and stirred thoroughly to obtain dispersion I. The dispersion I was treated with an ultrasonic cell crusher with a power of 700 W for 5 h, and then post-treated (centrifugal separation, drying) to obtain sulfur-doped gC 3 N 4 Nanosheets; wherein sulfur-doped gC 3 N 4 The mass ratio of micron sheets to deionized water is 10:2;

[0216] Sulfur-doped gC 3 N 4 The diameter of the nanosheets is 200-300 nm;

[0217] (3) The sulfur-doped gC prepared in step (2) 3 N 4 The nanosheets were dispersed in the copper salt solution and stirred for 30 min. Then, they were stirred at 800 r / min for 10 min under the irradiation of a 700 W xenon lamp. Then, they were washed three times by centrifugation with deionized water and ethanol respectively, and then dried in a vacuum oven at 60 ° C for 12 h to obtain Cu-loaded sulfur-doped gC. 3 N 4 Composite material; wherein sulfur-doped gC 3 N 4 The ratio of nanosheets to copper salt solution was 10 mg:2 mL.

[0218] The final Cu-loaded sulfur-doped gC 3 N 4 The composite material has a crystalline-amorphous heterojunction structure, which is composed of crystalline sulfur-doped gC 3 N 4 The nanosheets are composed of amorphous Cu nanoclusters uniformly loaded on the surface. The particle size of the Cu nanoclusters is 7-9nm, and the loading amount of the Cu nanoclusters is 16wt%. 3 N 4 The photocurrent density of the composite material is 2.1 μA cm -2 .

[0219] Cu-loaded sulfur-doped gC 3 N 4 Application of composite materials: the Cu prepared above is loaded with sulfur-doped gC 3 N 4 The composite material was dispersed in water to obtain a dispersion II with a concentration of 1 mg / mL. The bacterial solution (containing 10 6 CFU / mL Escherichia coli), the volume ratio of dispersion II to bacterial solution was 1:1, and the cells were incubated at 36°C under visible light for 18 h.

[0220] The above test shows that after the dispersion II with the bacterial solution was left to stand for 6 hours, the survival rate of E. coli was 0%, and the E. coli was completely killed. Therefore, the Cu-loaded sulfur-doped gC prepared above 3 N 4 The composite material has significant photocatalytic bactericidal properties.

[0221] Embodiment 11

[0222] A Cu-loaded sulfur-doped gC 3 N 4 The preparation method of the composite material comprises the following steps:

[0223] (1) Preparation of raw materials;

[0224] C 3 N 4 Precursor: a mixture of melamine (CAS No.: 108-78-1) and urea (CAS No.: 57-13-6) in a mass ratio of 1:1;

[0225] Sulfur source: a mixture of thiourea (CAS No.: 62-56-6) and thioacetamide (CAS No.: 62-55-5) in a mass ratio of 1:1;

[0226] Deionized water;

[0227] Copper salt solution: the solute is a mixture of copper sulfate (CAS No.: 7758-99-8) and copper nitrate (CAS No.: 10031-43-3) in a mass ratio of 1:1, the solvent is deionized water, and the concentration is 6M;

[0228] Ethanol;

[0229] (2) Preparation of sulfur-doped gC 3 N 4 Nanosheets;

[0230] (2.1) The mass ratio of gC is 10:3. 3 N 4 The precursor and the sulfur source were ground in a mortar for 20 minutes to mix evenly, and then placed in a porcelain boat, heated to 450°C in a muffle furnace at a heating rate of 6°C / min and kept warm for 6 hours, and then ground again. After grinding, the temperature was raised to 600°C in a muffle furnace at a heating rate of 8°C / min and kept warm for 8 hours to obtain sulfur-doped gC 3 N 4 Micron sheet;

[0231] (2.2) The sulfur-doped gC 3 N 4The micronized flakes were dispersed in deionized water and stirred thoroughly to obtain dispersion I. The dispersion I was treated with an ultrasonic cell crusher with a power of 600 W for 2 h, and then post-treated (centrifugal separation, drying) to obtain sulfur-doped gC 3 N 4 Nanosheets; wherein sulfur-doped gC 3 N 4 The mass ratio of micron sheets to deionized water is 10:3;

[0232] Sulfur-doped gC 3 N 4 The diameter of the nanosheets is 450-600 nm;

[0233] (3) The sulfur-doped gC prepared in step (2) 3 N 4 The nanosheets were dispersed in the copper salt solution and stirred for 30 min. Then, they were stirred at a rate of 100 r / min for 40 min under the irradiation of a 100 W xenon lamp. Then, they were washed three times by centrifugation with deionized water and ethanol respectively, and then dried in a vacuum oven at 60 ° C for 12 h to obtain Cu-loaded sulfur-doped gC 3 N 4 Composite material; wherein sulfur-doped gC 3 N 4 The ratio of nanosheets to copper salt solution was 10 mg:6 mL.

[0234] The final Cu-loaded sulfur-doped gC 3 N 4 The composite material has a crystalline-amorphous heterojunction structure, which is composed of crystalline sulfur-doped gC 3 N 4 The nanosheets are composed of amorphous Cu nanoclusters uniformly loaded on the surface. The particle size of the Cu nanoclusters is 11-14nm, and the loading amount of the Cu nanoclusters is 34wt%. 3 N 4 The photocurrent density of the composite material is 2.5 μA cm -2 .

[0235] Cu-loaded sulfur-doped gC 3 N 4 Application of composite materials: the Cu prepared above is loaded with sulfur-doped gC 3 N 4 The composite material was dispersed in water to obtain a dispersion II with a concentration of 5 mg / mL. The bacterial solution (containing 10 8 CFU / mL Escherichia coli), the volume ratio of dispersion II to bacterial solution was 1:0.8, and the samples were allowed to stand at 28°C under visible light for 18 h.

[0236] The above test shows that after the dispersion II with the bacterial solution was left to stand for 6 hours, the survival rate of E. coli was 0%, and the E. coli was completely killed. Therefore, the Cu-loaded sulfur-doped gC prepared above 3 N 4 The composite material has significant photocatalytic bactericidal properties.

[0237] Example 12

[0238] A Cu-loaded sulfur-doped gC 3 N 4 The preparation method of the composite material comprises the following steps:

[0239] (1) Preparation of raw materials;

[0240] C 3 N 4 Precursor: melamine, CAS number: 108-78-1;

[0241] Sulfur source: ammonium sulfate, CAS number: 7783-20-2;

[0242] Deionized water;

[0243] Copper salt solution: the solute is copper nitrate, CAS number: 10031-43-3, the solvent is deionized water, the concentration is 3M;

[0244] Ethanol;

[0245] (2) Preparation of sulfur-doped gC 3 N 4 Nanosheets;

[0246] (2.1) The mass ratio of gC is 10:3. 3 N 4 The precursor and the sulfur source were ground in a mortar for 20 minutes and mixed evenly, then placed in a porcelain boat, heated to 500°C in a muffle furnace at a heating rate of 1°C / min and kept warm for 7 hours, and then ground again. After grinding, the temperature was raised to 570°C in a muffle furnace at a heating rate of 3°C / min and kept warm for 4 hours to obtain sulfur-doped gC 3 N 4 Micron sheet;

[0247] (2.2) The sulfur-doped gC 3 N 4 The micronized flakes were dispersed in deionized water and stirred thoroughly to obtain dispersion I. The dispersion I was treated with an ultrasonic cell crusher with a power of 1300 W for 3 h, and then post-treated (centrifugal separation, drying) to obtain sulfur-doped gC 3 N 4 Nanosheets; wherein sulfur-doped gC 3 N4 The mass ratio of micron sheets to deionized water is 10:7;

[0248] Sulfur-doped gC 3 N 4 The diameter of the nanosheets is 100-200 nm;

[0249] (3) The sulfur-doped gC prepared in step (2) 3 N 4 The nanosheets were dispersed in the copper salt solution and stirred for 30 min. Then, they were stirred at 400 r / min for 30 min under the irradiation of a 500 W xenon lamp. Then, they were washed three times by centrifugation with deionized water and ethanol respectively, and then dried in a vacuum oven at 60 ° C for 12 h to obtain Cu-loaded sulfur-doped gC 3 N 4 Composite material; wherein sulfur-doped gC 3 N 4 The ratio of nanosheets to copper salt solution was 10 mg:6 mL.

[0250] The final Cu-loaded sulfur-doped gC 3 N 4 The composite material has a crystalline-amorphous heterojunction structure, which is composed of crystalline sulfur-doped gC 3 N 4 The nanosheets are composed of amorphous Cu nanoclusters uniformly loaded on the surface. The particle size of the Cu nanoclusters is 17-20nm, and the loading amount of the Cu nanoclusters is 38wt%. 3 N 4 The photocurrent density of the composite material is 2.3 μA cm -2 .

[0251] Cu-loaded sulfur-doped gC 3 N 4 Application of composite materials: the Cu prepared above is loaded with sulfur-doped gC 3 N 4 The composite material was dispersed in water to obtain a dispersion II with a concentration of 0.01-5 mg / mL. The bacterial solution (containing 10 6 CFU / mL Escherichia coli), the volume ratio of dispersion II to bacterial solution was 1:0.1~10, and the samples were placed at 38°C under visible light for 18 h.

[0252] The above test shows that after the dispersion II with the bacterial solution was left to stand for 6 hours, the survival rate of E. coli was 0%, and the E. coli was completely killed. Therefore, the Cu-loaded sulfur-doped gC prepared above 3 N 4 The composite material has significant photocatalytic bactericidal properties.

Claims

1. A Cu-loaded sulfur-doped g-C3N4 composite material, characterized in that: It has a crystalline-amorphous heterojunction structure, including crystalline sulfur-doped g-C3N4 nanosheets and amorphous Cu nanoclusters uniformly loaded on the surface thereof, the diameter of the sulfur-doped g-C3N4 nanosheets is 100-600nm, the particle size of the Cu nanoclusters does not exceed 20nm, and the loading amount of the Cu nanoclusters is 3-50wt%; The preparation method of Cu-loaded sulfur-doped g-C3N4 composite material is as follows: Cu nanoclusters are loaded on sulfur-doped g-C3N4 nanosheets by a photoreduction method to obtain a Cu-loaded sulfur-doped g-C3N4 composite material. The specific process is as follows: sulfur-doped g-C3N4 nanosheets are dispersed in a copper salt solution, stirred to react under xenon light illumination, and post-treated to obtain a Cu-loaded sulfur-doped g-C3N4 composite material.

2. A Cu-loaded sulfur-doped g-C3N4 composite material according to claim 1, characterized in that: The photocurrent density of Cu-loaded sulfur-doped g-C3N4 composites is 1.8~3.2 μA cm -2 .

3. The Cu-loaded sulfur-doped g-C3N4 composite material according to claim 1, characterized in that: The ratio of sulfur-doped g-C3N4 nanosheets to copper salt solution is 10 mg: 1~10 mL; the concentration of the copper salt solution is 1~10 M; the copper salt is one or more of copper chloride, copper sulfate, copper nitrate, basic copper carbonate and basic copper sulfate; the power of the xenon lamp is 50~1000 W; the stirring reaction time is 10~60 min, and the rate is 100~800 r / min.

4. The Cu-loaded sulfur-doped g-C3N4 composite material according to claim 1, characterized in that: The preparation process of sulfur-doped g-C3N4 nanosheets is as follows: first, sulfur-doped g-C3N4 micron sheets are prepared by thermal decomposition, and then the sulfur-doped g-C3N4 micron sheets are crushed to obtain sulfur-doped g-C3N4 nanosheets.

5. The Cu-loaded sulfur-doped g-C3N4 composite material according to claim 4, characterized in that: The specific process of preparing sulfur-doped g-C3N4 micron sheets by pyrolysis is as follows: after the g-C3N4 precursor and the sulfur source are evenly mixed, the first pyrolysis treatment, grinding, and the second pyrolysis treatment are sequentially performed to obtain sulfur-doped g-C3N4 micron sheets; the mass ratio of the g-C3N4 precursor to the sulfur source is 10:1~5; the g-C3N4 precursor is one or more of melamine, urea, trichloromelamine and dicyandiamide; the sulfur source is one or more of thioacetamide, thiourea, sulfur powder and sulfur-containing inorganic salts; the heating rate of the first pyrolysis treatment or the second pyrolysis treatment is 1~10℃ / min, the heating end point is 450~600℃, and the insulation time is 2~8h.

6. The Cu-loaded sulfur-doped g-C3N4 composite material according to claim 4, characterized in that: The specific process of crushing the sulfur-doped g-C3N4 micron sheets is as follows: disperse the sulfur-doped g-C3N4 micron sheets in deionized water, fully stir and mix to obtain a dispersion, treat the dispersion with an ultrasonic cell crusher, and then perform post-treatment; the mass ratio of the sulfur-doped g-C3N4 micron sheets to deionized water is 10:1~10; the power of the ultrasonic cell crusher is 500~1500W; the treatment time is 1~5h.

7. Use of a Cu-loaded sulfur-doped g-C3N4 composite material as claimed in claim 1 or 2, characterized in that: Used as a photocatalyst to kill microorganisms.