Tellurite glass and its preparation method and application
By using lanthanum oxide to replace SrF2 in tellurite glass and adjusting the contents of ZnO and Nb2O5, the problem of insufficient excitation wavelength and thermal stability is solved, achieving more efficient luminous performance and thermal stability, suitable for high-power LEDs and Laser lighting devices.
Patent Information
- Application Number
- CN202410526847.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-29
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-04-29
AI Technical Summary
Existing tellurite glass has deficiencies in excitation wavelength and thermal stability, making it difficult to meet the luminous performance requirements of high-power LEDs and laser lighting in high-temperature environments.
By replacing the original SrF2 with lanthanum oxide (La2O3) and adjusting the contents of zinc oxide (ZnO) and rhenium oxide (Nb2O5), 60mol% tellurium oxide-0.5mol% dysprosium oxide- The glass system of 5 mol% lanthanum oxide-20~30 mol% zinc oxide-5~15 mol% rhenium oxide is prepared by high-temperature melting-rapid quenching method, and is cold quenched and thermally stabilized during the annealing process.
It significantly improves the excitation wavelength and thermal stability of the glass, reduces the optical band gap, enhances the quantum luminescence efficiency of rare earth ions and the anti-crystallization ability of the glass, and is suitable for high-power LED and laser lighting applications.
Smart Images

Figure CN118373589B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of special glass, and in particular to tellurite glass and a preparation method and application thereof. Background Art
[0002] With the expansion of application demand for high-power white light sources in high-brightness lighting, laser lighting, laser display and other fields, as well as the development of high-power blue light chips and laser diodes, solid-state light-emitting materials have ushered in new challenges.
[0003] At present, the commercial packaging method of white light LED (Light Emitting Diode) and LD (Laser Didoe) is to mix the fluorescent conversion material and organic resin. High-power LED and white light LD devices will generate a lot of heat during operation, and the organic fluorescent material has low thermal conductivity and poor heat resistance, which will cause the light conversion material in the form of "phosphor + organic resin" to fail to emit light. Rare earth ion-doped glass materials have uniform photoluminescent properties, low synthesis price, excellent chemical resistance and thermal stability. Therefore, replacing the organic epoxy resin or silicone layer with rare earth ion-doped glass can effectively solve the problem of light failure caused by high temperature.
[0004] At present, rare earth ions can emit a variety of colors due to their df, ff electronic transitions. 3+ ) ions can emit red ( 4 F 9 / 2 → 6 H 11 / 2 , 665nm), yellow ( 4 F 9 / 2 → 6 H 13 / 2 , 576nm), blue ( 4 F 9 / 2 → 6 H 15 / 2 , 484nm) three colors of visible light, satisfying the red-yellow-blue (RYB) scheme, so dysprosium ions occupy an important position in white light emission.
[0005] Tellurite glass has the characteristics of high refractive index, good rare earth ion solubility and large laser damage threshold, and is an important material for the development of high-power LEDs and laser lighting. However, the structure of pure TeO2 glass is unstable, and the use of additional modifier ions (such as titanium, zinc, calcium, etc.) can effectively improve the glass forming ability and stability. SrF2 can be used as a glass forming aid to help inhibit the crystallization of glass. In addition, SrF2 can reduce the free OH in the glass. - , improve the quantum luminescence efficiency of rare earth ions.
[0006] In the previous patent application of the present applicant (CN2024101095534, Tellurite glass and its preparation method and application), the relationship between Nb and Zn was studied;
[0007] This scheme uses tellurium oxide, dysprosium oxide, strontium fluoride, zinc oxide, and niobium oxide as raw materials to prepare tellurite glass.
[0008] The problem with this glass is that the excitation wavelength and thermal stability need to be improved. Summary of the invention
[0009] The object of the present invention is to provide a tellurite glass, which has effectively improved excitation wavelength and thermal stability performance compared with the tellurite glass in the prior application.
[0010] At the same time, the present invention also provides a preparation method and application of the tellurite glass.
[0011] The specific scheme of the present invention is:
[0012] A tellurite glass comprising the following molar percentage components:
[0013] Tellurium oxide 60%;
[0014] Dysprosium oxide 0.5%;
[0015] Lanthanum oxide 5%;
[0016] Zinc oxide 20-30%;
[0017] Niobium oxide 5-15%.
[0018] The above-mentioned tellurite glass includes the following molar percentage components:
[0019] Tellurium oxide 60%;
[0020] Dysprosium oxide 0.5%;
[0021] Lanthanum oxide 5%;
[0022] Zinc oxide 25-27.5%;
[0023] Niobium oxide 7.5-10%.
[0024] The above-mentioned tellurite glass includes the following molar components:
[0025] Tellurium oxide 60 mol;
[0026] Dysprosium oxide 0.5 mol;
[0027] Lanthanum oxide 5 mol;
[0028] Zinc oxide 27.5 mol;
[0029] Niobium oxide 7.5 mol;
[0030] or,
[0031] Tellurium oxide 60 mol;
[0032] Dysprosium oxide 0.5 mol;
[0033] Lanthanum oxide 5 mol;
[0034] Zinc oxide 25 mol;
[0035] Niobium oxide 10 mol.
[0036] At the same time, the present invention also discloses a method for preparing any of the above-mentioned tellurite glass, comprising crushing and uniformly mixing the raw materials, keeping the raw materials warm in a high-temperature resistance furnace at 1000-1100°C for 30-50 minutes to melt the raw materials into glass liquid, then pouring the molten glass liquid onto a preheated brass plate to quench the glass liquid to form glass; then keeping the glass warm in an annealing furnace at 300-400°C for 6-10 hours; and cooling to room temperature after annealing.
[0037] In the above-mentioned tellurite glass method, the raw materials are crushed and mixed evenly, and then kept warm in a high-temperature resistance furnace at 1100°C for 30 minutes to melt the raw materials into glass liquid, and then the molten glass liquid is poured onto a preheated brass plate to quench the glass liquid to form glass; the glass is then kept warm in an annealing furnace at 350°C for 8 hours; after annealing, it is naturally cooled to room temperature.
[0038] At the same time, the present invention also discloses the use of any of the above-mentioned tellurite glasses to prepare optical fibers.
[0039] At the same time, the present invention also discloses the use of any of the above-mentioned tellurite glasses to prepare laser lighting glass.
[0040] At the same time, the present invention also discloses the use of any of the above-mentioned tellurite glasses to prepare laser display elements.
[0041] At the same time, the present invention also discloses the use of any of the above-mentioned tellurite glasses to prepare LED light-emitting elements.
[0042] The beneficial effects of this application are:
[0043] The present invention adopts lanthanum oxide to replace SrF2 in the original solution, and its excitation wavelength and thermal stability performance are effectively improved.
[0044] The mechanism is that using La2O3 to replace SrF2 in the original solution can effectively increase the effective molar oxygen in the glass system, promote the transformation of the network structure, make the ligands in the glass bond to each other to form a network structure, and improve the stability of the glass. In addition, La2O3 can reduce the optical band gap of the glass, making rare earth ions easier to excite. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 is the excitation spectrum of TSZN7.5 and TZNL2 in the range of 300-500nm;
[0046] Figure 2 is the emission spectrum of Dy3+-doped TZNL glass (λex=452nm);
[0047] Figure 3 This is the DSC curve of Dy3+ doped TZNL glass. DETAILED DESCRIPTION
[0048] The present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. In the description of the present invention, it should be noted that, if no specific conditions are specified in the embodiments, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0049] Part I Preparation of Tellurites
[0050] The composition and nomenclature of the tellurite glass series with different Nb2O5 contents are shown in Table 1.
[0051] Each glass sample is made of 6g of raw materials, all of which have a purity of 99.99%. The materials are then weighed accurately according to the designed molar composition.
[0052] In this experiment, the synthesis method selected is high temperature melting-rapid quenching method.
[0053] The preparation process is as follows:
[0054] 1. First accurately weigh 6g of raw material.
[0055] 2. In a dry air atmosphere, mix the raw materials of each sample thoroughly.
[0056] 3. Pour the fully ground and mixed raw materials into a corundum crucible, and then place it in a high-temperature resistance furnace at 1100°C for 30 minutes.
[0057] 4. Pour the molten glass onto a preheated brass plate and quickly quench it to form transparent glass. Then, keep it in an annealing furnace at 350°C for 8 hours. After annealing, let it cool down slowly until it reaches room temperature.
[0058] 5. Use an automatic precision grinding and polishing machine to grind and polish both sides of the sample to obtain glass slices with a thickness of 2 mm.
[0059] Table 1 Composition and naming of glass samples
[0060]
[0061]
[0062] The density of the glass samples was measured by the Archimedean drainage method, and the results are shown in Table 1. The refractive index of the glass was measured by the prism minimum deflection method. The thermal stability of the matrix glass was measured by a STA 449F5 synchronous TG-DSC thermal analyzer (NETZSCH, Germany) at a heating rate of 10 K / min. The fluorescence spectrum of the glass in the range of 450-700 nm was measured by F-7000 (Hitachi, Japan) All the above tests were carried out at room temperature.
[0063] Part II Performance Testing and Result Analysis
[0064] 2.1 Photoluminescence mechanism
[0065] By monitoring Dy 3+ The characteristic emission peak λ em =576nm, TSZN7.5 was obtained
[0066] The excitation spectra of (60TeO2-27.5ZnO-5SrF2-0.5Dy2O3-7.5Nb205) and TZNL2 in the range of 300-500nm, such as Figure 1 As shown. In the figure, six transition excitation bands from 6H15 / 2 to 6P7 / 2, 4P3 / 2, 4I13 / 2, 4G11 / 2, 4I15 / 2 and 6F9 / 2 are observed, which are located near 351, 365, 388, 427, 452 and 475nm respectively. In addition, it can be seen that compared with TSZN7.5, the best excitation peak of TZNL2 is red-shifted to 452nm. This is because after replacing SrF2 with La2O3, its optical band gap is reduced, making Dy2O3 easily activated by photons with lower energy.
[0067] The fluorescence spectrum of ZNLx glass under 452nm light excitation is 460~620nm, such as Figure 2The main emission peaks are located at 481nm and 576nm, corresponding to the transitions of 4F9 / 2→6H15 / 2 and 4F9 / 2→6H13 / 2, respectively. Studies have shown that Nb 5+ The incorporation of Nb2O5 affects the luminescence properties of Dy3+ doped glass. When Nb2O5 is at a low concentration, the emission intensity of Dy3+ increases with the increase of Nb2O5 content, reaching the highest value at 7.5% (wt). This enhancement may be due to the smaller Nb 5+ (ionic radius 64pm) replaced Zn 2+ (ion radius 74pm), increasing the number of Dy3+ in the glass lattice. However, as the concentration of Nb2O5 continues to increase, the emission intensity decreases because the distance between Dy3+ decreases and the interaction strengthens, resulting in an increase in the probability of non-radiative transitions, which in turn reduces the luminescence efficiency.
[0068] 2.2 Thermal stability test
[0069] Figure 3 The DSC curves of tellurite glasses containing different amounts of Nb2O5 are shown, with the glass transition temperature (Tg), crystallization start temperature (Tx), and crystallization temperature (Tp) marked. The ΔT (Tx-Tg) of these glasses are all over 150°C, indicating that they have good thermal stability and anti-crystallization ability, and are suitable for high-power LED and white light LD fields. With the increase of Nb2O5 content, Tg, Tx, and ΔT all increase. When the Nb2O5 content reaches 7.5% (wt), these values reach the maximum, indicating that the addition of Nb2O5 effectively improves the thermal stability and anti-crystallization of the glass.
[0070] Summarize:
[0071] 1. Using La2O3 instead of SrF2 effectively reduces the optical band gap of the glass system, making Dy3+ more easily activated by low-energy photons.
[0072] 2. By changing the content of ZnO and Nb2O5, the luminescence performance of Dy3+ in the visible light band can be regulated. When the content of Nb2O5 reaches 7.5%, the luminescence performance is optimal.
[0073] 3. In the TeO2-ZnO-Nb2O5-La2O3-Dy2O3 glass system, increasing the content of Nb2O5 increases the number of effective oxygen atoms inside the glass system. Microscopic chemical bonds form a network to enhance its thermal stability, which is more conducive to its application in high-power lighting devices.
Claims
1. A tellurite glass, characterized in that: It is composed of the following molar components: Tellurium oxide 60 mol; Dysprosium oxide 0.5 mol; Lanthanum oxide 5 mol; Zinc oxide 27.5 mol; Niobium oxide 7.5 mol; or, Tellurium oxide 60 mol; Dysprosium oxide 0.5 mol; Lanthanum oxide 5 mol; Zinc oxide 25 mol; Niobium oxide 10 mol.
2. A method for preparing the tellurite glass according to claim 1, characterized in that: The raw materials are crushed and mixed evenly, and kept warm in a high-temperature resistance furnace at 1000-1100°C for 30-50 minutes to melt the raw materials into glass liquid, and then the molten glass liquid is poured onto a preheated brass plate to quench the glass liquid to form glass; the glass is then kept warm in an annealing furnace at 300-400°C for 6-10 hours; after annealing, the temperature is lowered to room temperature.
3. The method of producing tellurite glass according to claim 2, characterized in that: The raw materials are crushed and mixed evenly, and kept warm in a high-temperature resistance furnace at 1100°C for 30 minutes to melt the raw materials into glass liquid. The molten glass liquid is then poured onto a preheated brass plate to quench the glass liquid to form glass. The glass is then kept warm in an annealing furnace at 350°C for 8 hours. After annealing, the temperature is naturally lowered to room temperature.
4. Use of the tellurite glass as claimed in claim 1 in preparing optical fiber.
5. Use of the tellurite glass according to claim 1 to prepare laser lighting glass.
6. Use of the tellurite glass according to claim 1 in preparing laser display elements.
7. Use of the tellurite glass as claimed in claim 1 to prepare LED light-emitting elements.
Citation Information
Patent Citations
Tellurate glass as well as preparation method and application thereof
CN117964233A
Tellurate glass and its application
CN1597584A