A partially filled warm mix SBS composite modified asphalt and preparation method thereof

By optimizing the formula and process, partially filled warm-mix SBS composite modified asphalt is used, and waste cooking oil and other modifiers are used to solve the complex and high-cost problems of existing warm-mix asphalt technology and achieve high temperature stability and low temperature resistance. It is crack-resistant and suitable for areas with large temperature differences, reducing production costs and harmful emissions.

CN118374164BActive Publication Date: 2024-10-15TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410641596.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-22
Publication Date
2024-10-15
Estimated Expiration
2044-05-22

AI Technical Summary

Technical Problem

The existing warm-mix asphalt technology has complex production methods, high costs, poor high and low temperature performance, and is not suitable for areas with large temperature differences.

Method used

Partially filled warm-mix SBS composite modified asphalt is used. By optimizing the formula and preparation process, using waste cooking oil, viscosity reducer, gel agent and antifreeze, a low-viscosity process is designed to improve the high-temperature stability and low-temperature resistance of the asphalt. fission.

Benefits of technology

Significantly reduces the viscosity of asphalt, improves rutting resistance and low-temperature performance, lowers production and construction temperatures, reduces harmful gas emissions, realizes resource recycling, extends the service life of asphalt, and improves the overall quality of the road .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118374164B_ABST
    Figure CN118374164B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of warm-mix asphalt pavement materials, and specifically discloses a partially filled warm-mix SBS composite modified asphalt suitable for warm-mix asphalt pavement and a preparation method thereof. It is composed of the following raw materials: 100 parts of SBS modified asphalt, 1 to 2 parts of gelling agent, 5 to 8.3 parts of waste cooking oil, 1 to 1.7 parts of viscosity reducer, 3 parts of antifreeze agent and 0.1 part of stabilizer. The specific preparation method is as follows: waste cooking oil, viscosity reducer and gelling agent are mixed to obtain a partially filled pre-gel warm-mix modifier; partially filled pre-gel warm-mix modifier, antifreeze agent, stabilizer and SBS modified asphalt are mixed to obtain a partially filled warm-mix SBS composite modified asphalt. The partially filled warm-mix SBS composite modified asphalt prepared by the present invention optimizes the construction efficiency through the design of low viscosity, and at the same time exhibits excellent high temperature stability and low temperature crack resistance. It is particularly suitable for areas with large temperature differences, and provides strong support and guarantee for transportation construction in cold areas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of warm-mix asphalt pavement materials, and in particular relates to a partially filled warm-mix SBS composite modified asphalt suitable for warm-mix asphalt pavement and a preparation method thereof. Background Art

[0002] As my country's requirements for building low-carbon transportation continue to increase, the demand for energy-saving and emission-reducing road construction materials is also increasing. The use of warm mix technology can reduce consumption, reduce the emission of harmful gases such as asphalt smoke, and reduce the aging of asphalt during construction. Compared with the same type of hot mix asphalt mixture, the former can reduce the mixing temperature of the mixture by about 20℃-40℃ while basically keeping the gradation, oil-stone ratio and construction process of the asphalt mixture unchanged, and the performance can also reach the new type of hot mix mixture. Based on existing research, we still lack economical and efficient warm mix asphalt technology, which limits our advancement in highway preventive maintenance management. Therefore, it is necessary to study a warm mix asphalt technology to solve this problem.

[0003] At present, waste cooking oil is widely used in the construction of road pavement. On the one hand, it is mainly used for the modification of asphalt, and on the other hand, it is used for the regeneration of aged asphalt. Various documents have shown that because waste cooking oil contains components similar to asphalt, it can be used as a regeneration agent for aged asphalt. At the same time, it will lead to an improvement in the low-temperature performance of asphalt, but will reduce the high-temperature performance of asphalt. Ethylene bisstearamide (EBS) is a wax-based warm mix agent. EBS is compatible with most waxes and plasticizers. The polarity of its two central amide groups and the non-polarity of its two fatty chains make this product an excellent surfactant that is compatible with almost all solvents and most polymer systems. The existing patent application (CN 115558303A) has proposed a better solution for asphalt viscosity reduction, but it has not shown good performance in terms of high and low temperature performance. Its more complicated preparation scheme and high market price are not widely applicable to existing pavements. The published patent application (CN 106751968A) proposes a method that can improve high and low temperature performance and reduce mixing viscosity, but its preparation is not economical and is not suitable for relatively cold northern cold areas with large temperature differences. Summary of the invention

[0004] The present invention is proposed to solve a series of problems such as the complicated production method of the existing warm mix modified asphalt, high growth cost, poor high and low temperature performance, etc.

[0005] The purpose of the present invention is to develop a partially filled warm mix SBS composite modified asphalt, solve the problems existing in traditional SBS modified asphalt by optimizing the formula and preparation process, and improve the performance of asphalt materials. The partially filled warm mix SBS composite modified asphalt prepared by the present invention optimizes the construction efficiency through the design of low viscosity, and at the same time shows excellent high temperature stability and low temperature crack resistance. It is particularly suitable for areas with large temperature differences, providing strong support and guarantee for transportation construction in cold areas.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A partially filled warm-mix SBS composite modified asphalt is composed of the following raw materials, measured by weight: 100 parts of SBS modified asphalt, 1 to 2 parts of gelling agent, 5 to 8.3 parts of waste cooking oil, 1 to 1.7 parts of viscosity reducer, 3 parts of antifreeze agent and 0.1 part of stabilizer.

[0008] Furthermore, the partially filled warm-mix SBS composite modified asphalt is composed of the following raw materials in parts by mass: 100 parts of SBS modified asphalt, 5 to 6.7 parts of waste cooking oil, 1 to 1.3 parts of viscosity reducer, 1 to 2 parts of gelling agent, 3 parts of antifreeze agent and 0.1 part of stabilizer; the gelling agent is composed of water, glycerin, Carbomer 940, a pH regulator and a preservative, wherein the pH regulator is sodium hydroxide, and the preservative is boric acid (the preparation method of the gelling agent is: 5g of Carbomer 940, 25g of glycerin and 150g of water are mixed, 2g of the pH regulator is mixed with 50g of water, and then slowly added to the above liquid and stirred, and then 0.1g of the preservative is added thereto to obtain a transparent gel, i.e., the gelling agent).

[0009] More preferably, the partially filled warm-mix SBS composite modified asphalt is composed of the following raw materials, by mass: 100 parts of SBS modified asphalt, 5 parts of waste cooking oil, 1 part of viscosity reducer, 1 to 2 parts of gelling agent, 3 parts of antifreeze agent and 0.1 part of stabilizer.

[0010] Furthermore, the viscosity reducer is a mixture of ethylene bisstearamide (EBS) and dibasic acid ester in a mass ratio of 2:1, the antifreeze agent is dioctyl phthalate, and the stabilizer is sulfur powder.

[0011] The present invention also discloses a method for preparing the partially filled warm mix SBS composite modified asphalt, which comprises the following steps in sequence:

[0012] 1) Mix the waste cooking oil, gelling agent and viscosity reducer, heat and stir evenly at 100-120° C., and then cool in an environment of -5° C. for 6-7 hours to obtain a partially filled pre-gel warm mix modifier;

[0013] 2) The SBS modified asphalt is placed in an asphalt tank with a stirring device and heated to 180-200° C., and the stirring device is turned on; the partially filled pre-gel warm mix modifier prepared in 1) is added to the above SBS modified asphalt, and sheared uniformly at 180-200° C. and 2000-3000 rpm (preferably for 30 minutes);

[0014] 3) maintaining the temperature at 180° C. to 200° C., adding antifreeze agent and stabilizer thereto, stirring evenly at 2000 to 3000 rpm to obtain partially filled warm-mixed SBS composite modified asphalt.

[0015] In the present invention, the combined use of EBS and waste cooking oil can significantly reduce the viscosity of asphalt, improve the anti-rutting ability of the mixture and have very good low-temperature performance, which to a certain extent makes up for the defects of waste cooking oil and EBS and provides feasibility for subsequent research.

[0016] Compared with the prior art, the advantages and beneficial effects of the present invention are:

[0017] 1) The homemade partially filled warm mix SBS composite modified asphalt of the present invention has excellent elasticity and ductility, and can effectively resist road cracking caused by temperature changes or vehicle loads. This helps to maintain the integrity and aesthetics of the road surface, reduce the frequency of maintenance and replacement, and improve the overall quality of the road.

[0018] 2) In the preparation process of modified asphalt, the traditional modification method is often to completely fill or change the performance of asphalt by adding a fixed proportion of modifiers. The concept of "partial filling" proposes a different modification strategy, that is, not by adding the maximum amount of modifier, but by precisely controlling the amount of modifier added to achieve the optimization of asphalt performance. This strategy can not only reduce production costs, but also achieve more precise performance regulation. The partially filled warm mix technology adopted in this application is to fill SBS modified asphalt with waste cooking oil, viscosity reducer, and gelling agent in a certain proportion, and combine warm mix technology to achieve significant environmental benefits in the production and construction of asphalt. This technology effectively reduces the temperature requirements during asphalt production and construction, thereby greatly reducing the emission of harmful gases, such as carbon dioxide, sulfide, etc., and has made positive contributions to improving air quality and protecting the atmospheric environment. In addition, the main material of the asphalt modifier is waste cooking oil. This innovative measure not only reduces production costs, but also realizes the recycling of resources. Waste cooking oil is scientifically treated and converted into high-performance asphalt modifiers, which not only reduces dependence on new resources, but also avoids the pollution to the environment caused by improper treatment of waste oil. The application of this material not only saves resources but also complies with the concept of sustainable development, demonstrating our dual pursuit of environmental protection and economic benefits in the field of road construction.

[0019] 3) The use of gelling agent can absorb the light components with smaller molecular weight in waste cooking oil. This absorption process can improve the microstructure of asphalt, thereby optimizing its physical and chemical properties, such as improving the high temperature stability and anti-aging performance of asphalt. At the same time, the gelling agent can protect the asphalt components from the storage solvent to prevent them from decomposing or deteriorating due to temperature changes. This helps to improve the storage stability of asphalt and extend its service life. The addition of gelling agent can improve the adhesion between asphalt and aggregate, thereby improving the water damage resistance of asphalt mixture. This is of great significance for improving the quality and durability of roads. Since the gelling agent can optimize the microstructure of asphalt, so that it can still maintain good performance at high temperatures, the construction temperature can be reduced. This can not only reduce energy consumption, but also help to extend the construction season and improve construction efficiency.

[0020] 4) Antifreeze can increase the flexibility and ductility of asphalt, making it more adaptable to temperature changes and stress changes. At the same time, it can slow down the aging of asphalt and reduce its degree of hardening and embrittlement. This helps to extend the service life of asphalt and reduce the frequency of maintenance and repair.

[0021] 5) The partially filled warm mix SBS composite modified asphalt of the present invention has been comprehensively improved in terms of high temperature performance, low temperature performance and viscosity. Waste cooking oil fills the microscopic voids, reduces the viscosity of the asphalt, and together with the SBS modified asphalt reduces the temperature sensitivity of the asphalt, and improves the performance stability at high temperatures. The viscosity reducer reduces the viscosity of the asphalt, making the composite modified asphalt easier to mix and construct. The gelling agent and stabilizer increase the cohesion and stability of the asphalt, and the antifreeze agent ensures the fluidity and frost resistance of the asphalt at low temperatures. The combined action of these components makes the partially filled warm mix SBS composite modified asphalt not only have good stability and durability at high temperatures, but also maintain fluidity and elasticity at low temperatures. The overall performance has been significantly improved, providing a more reliable material choice for road construction, and reflecting the comprehensive benefits of environmental protection, economy and technological innovation. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is an appearance diagram of the waste cooking oil used in the present invention;

[0023] Figure 2 This is an appearance diagram of ethylene bisstearamide (EBS) used in the present invention;

[0024] Figure 3 A flow chart of preparing partially filled warm mix SBS composite modified asphalt according to the present invention;

[0025] Figure 4 This is a fluorescence microscope image of the composite modified asphalt prepared in Example 1 of the present invention;

[0026] Figure 5This is a fluorescence microscope image of the composite modified asphalt prepared in Example 2 of the present invention;

[0027] Figure 6 This is a fluorescence microscope image of the composite modified asphalt prepared in Example 3 of the present invention;

[0028] Figure 7 This is a fluorescence microscope image of the composite modified asphalt prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0029] The applicant further describes the technical solution of the present invention in conjunction with specific embodiments below, but the scope of protection requested by the claims of the present invention is not limited to these embodiments.

[0030] In the following examples and comparative examples, the asphalt used is the finished product SBS modified asphalt produced by Shanxi Yutong Road Materials Co., Ltd., and its batch number is XW230618PM009;

[0031] The gel used is composed of water, glycerin, carbomer 940, a pH regulator and a preservative, wherein the pH regulator is sodium hydroxide and the preservative is boric acid. The preparation method is as follows: 5g of carbomer 940, 25g of glycerin and 150g of water are mixed, 2g of the pH regulator is mixed with 50g of water and then slowly added to the above liquid and stirred until the pH reaches 8, and then 0.1g of the preservative is added thereto to obtain a transparent gel.

[0032] The waste cooking oil used was purchased from Chengdu Benbang Luqiao New Materials Co., Ltd. Figure 1 The ethylene bis stearamide (EBS) used is EBS-SF, and its appearance is shown in Figure 2 The viscosity reducer used was a mixture of ethylene bisstearamide (EBS) and dibasic acid ester in a mass ratio of 2:1. The dibasic acid ester was purchased from Tianjin Huasheng Chemical Reagent Co., Ltd. The antifreeze used was dioctyl phthalate, and the stabilizer used was sulfur powder.

[0033] In the following examples and comparative examples, each mass portion was tested on a 2 g scale.

[0034] Example 1

[0035] A partially filled warm mix SBS composite modified asphalt is composed of the following raw materials by weight: 100 parts of SBS modified asphalt, 5 parts of waste cooking oil, 1 part of viscosity reducer, 1 part of gelling agent, 3 parts of antifreeze agent and 0.1 part of stabilizer. The preparation method thereof comprises the following steps:

[0036] 1) Weigh the following raw materials according to their mass proportions: 100 parts of SBS modified asphalt, 5 parts of waste cooking oil, 1 part of viscosity reducer, 1 part of gelling agent, 3 parts of antifreeze agent and 0.1 part of stabilizer for later use;

[0037] 2) 5 parts of waste cooking oil, 1 part of gelling agent and 1 part of viscosity reducer were mixed, heated at 100° C. and stirred with a glass rod for 5 minutes, and then cooled at -5° C. for 6 hours to obtain a partially filled pre-gel warm mix modifier;

[0038] 3) 100 parts of SBS modified asphalt were placed in an asphalt tank with a stirring device and heated to 180° C. The stirring device was turned on, and then the partially filled pre-gel warm mix modifier prepared in step 2) was added to the asphalt tank, and sheared at 180° C. and 2000 rpm for 30 min;

[0039] 4) The temperature in the asphalt tank was maintained at 180° C., 3 parts of antifreeze agent and 0.1 parts of stabilizer were added thereto, and the mixture was stirred at 3000 rpm for 30 minutes to obtain partially filled warm-mixed SBS composite modified asphalt.

[0040] Example 2

[0041] A partially filled warm mix SBS composite modified asphalt is composed of the following raw materials by weight: 100 parts of SBS modified asphalt, 6.7 parts of waste cooking oil, 1.3 parts of viscosity reducer, 1 part of gelling agent, 3 parts of antifreeze agent and 0.1 part of stabilizer. The preparation method is the same as that of Example 1.

[0042] Example 3

[0043] A partially filled warm mix SBS composite modified asphalt is composed of the following raw materials by weight: 100 parts of SBS modified asphalt, 8.3 parts of waste cooking oil, 1.7 parts of viscosity reducer, 1 part of gelling agent, 3 parts of antifreeze agent and 0.1 part of stabilizer. The preparation method is the same as that of Example 1.

[0044] Example 4

[0045] A partially filled warm mix SBS composite modified asphalt is composed of the following raw materials by weight: 100 parts of SBS modified asphalt, 5 parts of waste cooking oil, 1 part of viscosity reducer, 2 parts of gelling agent, 3 parts of antifreeze agent and 0.1 part of stabilizer. The preparation method is the same as that of Example 1.

[0046] Example 5

[0047] A partially filled warm mix SBS composite modified asphalt, which is composed of the following raw materials by weight: 100 parts of SBS modified asphalt, 6.7 parts of waste cooking oil, 1.3 parts of viscosity reducer, 2 parts of gelling agent, 3 parts of antifreeze agent and 0.1 parts of stabilizer. Its preparation method is the same as that of Example 1

[0048] Example 6

[0049] A partially filled warm mix SBS composite modified asphalt is composed of the following raw materials by weight: 100 parts of SBS modified asphalt, 8.3 parts of waste cooking oil, 1.7 parts of viscosity reducer, 2 parts of gelling agent, 3 parts of antifreeze agent and 0.1 parts of stabilizer. The preparation method is the same as that of Example 1.

[0050] Comparative Example 1

[0051] A SBS modified asphalt is composed of the following raw materials in parts by mass: 100 parts of SBS modified asphalt.

[0052] Comparative Example 2

[0053] A waste cooking oil SBS modified asphalt is composed of the following raw materials by weight: 100 parts of SBS modified asphalt, 5 parts of waste cooking oil, 3 parts of antifreeze and 0.1 parts of stabilizer. The preparation method thereof comprises the following steps:

[0054] 1) Place SBS modified asphalt into an asphalt tank with a stirring device, heat it to 180°C, and turn on the stirring device;

[0055] 2) Add 5 parts of waste cooking oil to 100 parts of heated SBS modified asphalt and shear for 30 minutes at 180°C and 2000 rpm;

[0056] 3) The temperature was maintained at 180° C., 3 parts of antifreeze agent and 0.1 parts of stabilizer were added thereto, and the mixture was stirred at 3000 rpm for 30 minutes to obtain waste cooking oil SBS modified asphalt.

[0057] Comparative Example 3

[0058] A waste cooking oil SBS modified asphalt is composed of the following raw materials by weight: 100 parts of SBS modified asphalt, 6.7 parts of waste cooking oil, 3 parts of antifreeze agent and 0.1 part of stabilizer. The preparation method is the same as that of Comparative Example 2.

[0059] Comparative Example 4

[0060] A waste cooking oil SBS modified asphalt is composed of the following raw materials by weight: 100 parts of SBS modified asphalt, 8.3 parts of waste cooking oil, 3 parts of antifreeze agent and 0.1 part of stabilizer. The preparation method is the same as that of Comparative Example 2.

[0061] Comparative Example 5

[0062] An SBS modified asphalt with a viscosity reducer added is composed of the following raw materials by weight: 100 parts of SBS modified asphalt, 2 parts of viscosity reducer and 0.1 parts of stabilizer. The preparation method is the same as that of Comparative Example 2. The waste cooking oil in the formula is replaced with the viscosity reducer and the antifreeze agent is not added.

[0063] Comparative Example 6

[0064] A partially filled warm mix SBS composite modified asphalt is composed of the following raw materials by weight: 100 parts of SBS modified asphalt, 5 parts of waste cooking oil, 1 part of viscosity reducer, 1 part of gelling agent, 3 parts of antifreeze agent and 0.1 part of stabilizer. The preparation method is the same as that of Example 1. Compared with Example 1, the formula uses a different gelling agent, which is linear SBS, and its model is YH-791E.

[0065] Comparative Example 7

[0066] A partially filled warm mix SBS composite modified asphalt is composed of the following raw materials by weight: 100 parts of SBS modified asphalt, 5 parts of waste cooking oil, 1 part of viscosity reducer, 1 part of gelling agent and 0.1 part of stabilizer. The preparation method is the same as that of Example 1. Compared with Example 1, the formula does not add antifreeze.

[0067] The performance results of the composite modified asphalt prepared in the above examples and comparative examples are shown in Table 1:

[0068] Table 1 Composite modified asphalt performance test results

[0069]

[0070]

[0071] From Table 1, we can see that:

[0072] By comparing the data of Examples 1, 2, and 3 with Comparative Examples 2, 3, and 4, it is found that the addition of more waste cooking oil increases the penetration, decreases the softening point, and increases the ductility. The addition of a viscosity reducer can effectively neutralize these modification effects, and can reduce the penetration while increasing the softening point, and maintain an excellent 5°C ductility. Compared with the data in Comparative Example 1, it is not difficult to find that the composite modified asphalt in Examples 1 and 4 has an excellent softening point, that is, high temperature capability, and the composite modified asphalt in Examples 3 and 6 has an excellent 5°C ductility, that is, low temperature capability. From Comparative Example 5, it can be seen that although the modified asphalt with only a viscosity reducer has a higher softening point, its penetration and ductility are significantly reduced. This shows that the mixed use of waste cooking oil and a viscosity reducer can have good low temperature capabilities while maintaining high temperature performance. By comparing the data of Examples 1, 2, and 3 with Examples 4, 5, and 6, it is found that the use of more gelling agents has a small impact on the partially filled warm-mixed SBS composite modified asphalt. This is because the use of more gelling agent allows the light components to be absorbed, causing the modifier to harden, but its overall effect on the composite modified asphalt is small. By comparing Example 1 with Comparative Example 6, it is not difficult to find that after the gelling agent is replaced with linear SBS, its softening point and ductility will slightly increase, indicating that the addition of SBS has a good performance. The data of Example 1 and Comparative Example 7 show that the addition of antifreeze can significantly improve the low-temperature performance of the composite modified asphalt.

[0073] The viscosity values ​​of the asphalt samples of Examples 1 to 6 are significantly lower than those of Comparative Example 1. This result shows that the modified asphalt has better fluidity and a significant viscosity reduction effect, and the viscosity value is constantly decreasing with the increase in the amount of the modifier. Comparative Examples 2-4 show higher viscosity than Examples 1-3, which is because the mixture of EBS and divalent esters also has a significant viscosity reduction effect. It can be seen from Comparative Example 5 that adding 2 parts of viscosity reducer also has a good viscosity reduction ability, but its effect is not as significant as the viscosity reduction effect when waste cooking oil and viscosity reducer are used in combination. By comparing Example 1 with Comparative Example 6, it can be seen that after replacing the gelling agent with SBS, the viscosity value of the asphalt has increased significantly, which indicates that this example may not be suitable for warm mix asphalt.

[0074] Asphalt, as a significant temperature-sensitive material, needs to show excellent anti-rutting performance in summer to cope with deformation pressure under high temperature environment; and in winter, it must maintain excellent flexibility to ensure that the road surface is not easy to crack due to low temperature. Therefore, asphalt must have low temperature sensitivity to adapt to temperature changes in different seasons and ensure the durability and safety of the road surface. The viscosity-temperature index (VTS) is an indicator for evaluating the temperature sensitivity of asphalt. The larger the VTS value, the lower the temperature sensitivity of asphalt. By comparing the VTS value data with that of Comparative Example 1, it can be seen that the temperature sensitivity in Examples 2 and 5 is the highest, and the temperature sensitivity in Examples 1 and 4 is closest to that in Comparative Example 1. Comparative Examples 2-4 show that the addition of waste cooking oil will reduce the VTS value, but the VTS value will increase slightly with the increase of the amount of waste cooking oil. This is because although waste cooking oil will reduce the strength of asphalt, a large amount of waste cooking oil will soften asphalt, thereby reducing the temperature sensitivity. Comparative Example 5 shows that simply adding a viscosity reducer will increase the temperature sensitivity of asphalt. This is because the EBS in the viscosity reducer will form a crystalline network structure below its melting point, which will make the asphalt change more obviously with temperature. By comparing Examples 1, 2, and 3 with Comparative Examples 2-5, it can be seen that simply adding waste cooking oil or viscosity reducer increases the temperature sensitivity, but mixing the two has good temperature sensitivity, indicating the success of the design of partially filled warm-mix SBS composite modified asphalt.

[0075] In order to evaluate the effect of cooling medium on the rheological properties of asphalt, a bending beam rheometer (BBR) was used for testing. In the BBR experiment, the creep stiffness S≤300MPa and the creep rate m≥0.3 were used to evaluate the low temperature performance of asphalt. It can be seen from the BBR test data of Examples 1-3 that each example has good low temperature performance even at -24°C. Compared with Comparative Example 1, it can be seen that the addition of modifier improves the low temperature performance of the composite modified asphalt, and its low temperature crack resistance is also enhanced accordingly with the increase of the dosage. Although Comparative Examples 2-4 have lower S values ​​than Examples 1-3, that is, better low temperature performance, their softening points are relatively low. This feature suggests that their ability to resist rutting in high temperature environments is not outstanding, so they may not be suitable for high-performance pavements with strict requirements for high temperature anti-rutting performance. It can be seen from Comparative Example 5 that the addition of viscosity reducer significantly reduces the low temperature performance, but it can be seen from Examples 1-3 that the viscosity reducer has good low temperature performance after mixing with waste cooking oil, indicating that the two have good compatibility in this regard. Experimental Example 1 and Comparative Example 6 show that the addition of SBS slightly improves the low temperature performance, but this example is not used due to its higher viscosity.

[0076] Figure 4 , 5, 6, and 7 are microscopic microscope images of Examples 1-3 and Comparative Example 1, respectively. The green part in the fluorescent microscope is the asphalt phase, the bright part is the polymer phase, and the black part is the minority of non-fluorescent substances and bubbles contained in the asphalt. It can be seen from the figure that with the increase in the amount of modifier, the black substance in the original Comparative Example 1 is reduced, indicating that the modifier improves the compatibility of each polymer with asphalt. The reduction in polymer content indicates a reduction in viscosity in the asphalt, which shows that the viscosity reduction has achieved a significant effect. At the same time, the attached Figure 4-6 White floccules appeared in the asphalt, and the appearance of these structures reflects the high temperature performance of the asphalt. As the amount of modifier increases, the white floccules decrease, which also indicates that the high temperature performance of the asphalt deteriorates.

[0077] The performance improvement of partially filled warm mix SBS composite modified asphalt involves microstructure and chemical action. The SBS particles in SBS modified asphalt form a network structure with asphalt through physical crosslinking and adsorption, which improves the elasticity and toughness of asphalt. Impurities and unsaturated molecules in waste cooking oil fill the microscopic gaps in asphalt, reducing the friction between molecules and thus reducing the viscosity. The mixture of ethylene bisstearamide (EBS) and divalent acid esters in the viscosity reducer forms a microstructure in the asphalt, hindering the movement of asphalt molecules and reducing the viscosity of asphalt. Glycerol and carbomer 940 in the gelling agent form a gel-like structure in the asphalt, increasing the cohesion and adhesion of the asphalt. The stabilizer sulfur powder may delay the aging process of asphalt by inhibiting oxidation reactions. The antifreeze agent dioctyl phthalate prevents the freezing of asphalt at low temperatures and maintains its fluidity. Under the combined effect, the viscosity reduction effect, high temperature performance and low temperature performance of asphalt are significantly improved.

[0078] The performance test is described as follows:

[0079] The test procedures for asphalt and asphalt mixtures in highway engineering JTGE20-2011 shall be followed; specifically:

[0080] (1) Brookfield viscosity at 135°C / Pa·s: Executed in accordance with T0625; asphalt rotational viscosity test (Brookfield viscometer method);

[0081] (2) 25℃ needle penetration / mm: according to T0604; asphalt needle penetration test;

[0082] (3) 5℃ ductility / cm: according to T0605; asphalt ductility test;

[0083] (4) Softening point / ℃: According to T0606; Asphalt softening point test (ring and ball method);

[0084] (5) Viscosity-temperature index; according to T0628; asphalt rheological properties test (dynamic shear rheometer method);

[0085] (6) Creep stiffness S / MPa, creep rate m; according to T0627; asphalt bending creep stiffness test (bending beam rheometer method).

Claims

1. A method for preparing a partially filled warm mix SBS composite modified asphalt, wherein the partially filled warm mix SBS composite modified asphalt is composed of the following raw materials in parts by mass: 100 parts of SBS modified asphalt, 1-2 parts of gelling agent, 5-8.3 parts of waste cooking oil, 1-1.7 parts of viscosity reducer, 3 parts of antifreeze agent and 0.1 part of stabilizer; the gelling agent is composed of a mixture of water, glycerin, carbomer 940, a pH regulator and a preservative, wherein the pH regulator is sodium hydroxide and the preservative is boric acid; The viscosity reducer is a mixture of ethylene bisstearamide and dibasic acid ester in a volume ratio of 2:1, the antifreeze agent is dioctyl phthalate, and the stabilizer is sulfur powder; The preparation method comprises the following steps in sequence: 1) Mix the waste cooking oil, gelling agent and viscosity reducer, heat and stir evenly at 100-120° C., and then cool in an environment of -5° C. for 6-7 hours to obtain a partially filled pre-gel warm mix modifier; 2) The SBS modified asphalt is placed in an asphalt tank with a stirring device and heated to 180-200° C., and the stirring device is turned on; the partially filled pre-gel warm mix modifier prepared in 1) is added to the above SBS modified asphalt, and sheared uniformly at 180-200° C. and 2000-3000 rpm; 3) maintaining the temperature at 180° C. to 200° C., adding antifreeze agent and stabilizer thereto, stirring evenly at 2000 to 3000 rpm to obtain partially filled warm-mixed SBS composite modified asphalt.

2. The preparation method according to claim 1, characterized in that: The partially filled warm-mix SBS composite modified asphalt is composed of the following raw materials in parts by mass: 100 parts of SBS modified asphalt, 5 to 6.7 parts of waste cooking oil, 1 to 1.3 parts of viscosity reducer, 1 to 2 parts of gelling agent, 3 parts of antifreeze agent and 0.1 part of stabilizer.