A metal cobalt film and preparation method thereof
By combining CVD and ALD processes in cobalt film preparation, and using spray components to optimize the reaction space, the problems of uniformity and time efficiency in cobalt film preparation are solved, efficient and uniform cobalt film deposition is achieved, and the electrical performance is improved.
Patent Information
- Application Number
- CN202410813360.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-06-24
AI Technical Summary
In the existing cobalt film preparation process, the CVD method leads to poor uniformity within the chip, while the ALD method takes too long and is difficult to meet the stability and electrical performance requirements of small-size chip manufacturing.
Using CVD and ALD simultaneously, the cobalt source and reaction gas deposit a metallic cobalt film on the substrate, and the reduction reaction space of H2 and CCTBA is compressed through the spray component to reduce the inhomogeneity and gas phase diffusion effect in the reaction area. Improve deposition uniformity.
It achieves shortened growth time of cobalt thin film, improved in-chip growth uniformity and low film layer resistivity, improves the uniformity of the pressure field above the substrate, avoids uneven deposition caused by excessive pressure gradient, and improves film thickness Uniformity.
Smart Images

Figure CN118374791B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a metal cobalt film and a preparation method thereof. Background Art
[0002] With the continuous advancement of chip manufacturing technology, the characteristic size effect begins to become obvious in the size range below 10nm. In this case, the reduction in the size of metal wires will lead to an increase in the resistance of traditional interconnect materials such as copper, a decrease in signal transmission speed, and an increase in signal delay. Cobalt has fine grains, fewer grain boundaries, low resistance, and weak diffusion, which can better maintain the stability and electrical properties of the interconnect structure in small-size chip manufacturing. However, there are some problems in the preparation process of existing cobalt films, such as: the Co film prepared by chemical vapor deposition (CVD) has poor uniformity within the chip; it takes too long to prepare cobalt films by atomic layer deposition (ALD). Summary of the invention
[0003] In view of the above problems existing in the prior art, the present application provides a metal cobalt film and a preparation method thereof.
[0004] To solve the above problems, the present invention provides the following technical solutions:
[0005] In a first aspect, the present application provides a method for preparing a metal cobalt film, comprising: the method is applied in an inner cavity of a deposition device, a substrate is placed in the inner cavity, and the method uses CVD and ALD simultaneously to react a cobalt source and a reaction gas to deposit a metal cobalt film on the substrate.
[0006] In one embodiment of the present application, the deposition device is provided with 2 or more balanced carrier gas pipelines passing into the inner cavity, 1 or more CVD reaction gas and its carrier gas pipeline, and 1 or more ALD reaction gas and its carrier gas pipeline passing into the inner cavity through a plasma generator, and the balanced carrier gas pipeline is used as a CVD cobalt source and its carrier gas pipeline or an ALD cobalt source and its carrier gas pipeline when connected to a cobalt source, and at this time, the balanced carrier gas is used as a carrier gas for the CVD cobalt source or the ALD cobalt source;
[0007] In the method, the CVD reaction gas and its carrier gas pipeline, the ALD reaction gas and its carrier gas pipeline, the plasma generator, the CVD cobalt source and its carrier gas pipeline, the ALD cobalt source and its carrier gas pipeline, and the remaining balanced carrier gas pipelines except the CVD cobalt source and its carrier gas pipeline and the ALD cobalt source and its carrier gas pipeline are always kept in an open state. At the same time, the ALD cobalt source and its carrier gas pipeline and the ALD reaction gas and its carrier gas pipeline are opened or closed according to the needs of the ALD cycle. The ALD cycle includes: ALD cobalt source pulse, ALD cobalt source carrier gas purge, ALD reaction gas pulse, and ALD reaction gas carrier gas purge.
[0008] In one embodiment of the present application, the deposition equipment is further provided with an inert gas pipeline which passes into the inner cavity through a plasma generator, and the output port diameters of the inert gas pipeline, the CVD reaction gas and its carrier gas pipeline, the ALD reaction gas and its carrier gas pipeline, the CVD cobalt source and its carrier gas pipeline, the ALD cobalt source and its carrier gas pipeline and the remaining balance carrier gas pipelines are all the same; under this condition, the gas flow rates of the carrier gases of the CVD cobalt source and the ALD cobalt source and the remaining balance carrier gases are equal, the flow rates of the CVD cobalt source and the ALD cobalt source are equal, the carrier gas flow rates of the CVD reaction gas and the ALD reaction gas are equal, and the flow rates of the CVD reaction gas and the ALD reaction gas are equal.
[0009] In one embodiment of the present application, the inert gas pipeline is used to perform plasma pretreatment on the surface of the substrate.
[0010] In one embodiment of the present application, the preparation method further comprises annealing the metal cobalt film.
[0011] In one embodiment of the present application, the CVD and ALD are started one by one or simultaneously, and are shut down one by one or simultaneously.
[0012] In one embodiment of the present application, the CVD and ALD are started and shut down simultaneously, and the number of cycles of ALD deposition completed during the CVD period is not less than 1.
[0013] In one embodiment of the present application, the CVD cobalt source and the ALD cobalt source are CCTBA, the CVD reaction gas and the ALD reaction gas are H2, and the carrier gas of the CVD reaction gas and the ALD reaction gas, the remaining balance carrier gas and the inert gas are Ar.
[0014] In one embodiment of the present application, during the preparation of the metal cobalt film, the inner cavity deposition temperature is 100°C-200°C, and the cavity pressure of the inner cavity is 8torr-12torr during the CVD and ALD processes; the CVD reaction gas and ALD reaction gas H2 flow rates are 5000sccm respectively, the carrier gas Ar flow rates of the CVD reaction gas and the ALD reaction gas are 1000 sccm respectively, the CVD cobalt source and the ALD cobalt source CCTBA flow rates are 0-30 sccm respectively, the carrier gas flow rates of the CVD cobalt source and the ALD cobalt source and the remaining balance carrier gas Ar are 500 sccm, the plasma generator power is 1000W, and the cobalt source CCTBA temperature is 45°C.
[0015] In one embodiment of the present application, the time for one cycle of the ALD is 15s, including: the ALD cobalt source pulse time is 1s, that is, the ALD cobalt source turn-on time is 1s; the carrier gas purge time of the ALD cobalt source is 4s, that is, the ALD cobalt source turn-off time is 4s; the ALD reaction gas pulse time is 3s, that is, the ALD reaction gas turn-on time is 3s; the carrier gas purge time of the ALD reaction gas is 7s, that is, the ALD reaction gas turn-off time is 7s.
[0016] In one embodiment of the present application, a detachable spray assembly is provided in the inner cavity of the deposition device, and the spray assembly includes a columnar side wall and a first panel and a second panel connected to both ends of the columnar side wall, the columnar side wall has a thickness, and two or more ventilation pipes are dispersedly arranged in the columnar side wall, and one end opening of the ventilation pipe is located at an end of the columnar side wall close to the second panel, and a radial cobalt source delivery channel is provided at an end of the columnar side wall close to the first panel, and the cobalt source delivery channel is used to introduce a CVD cobalt source and its carrier gas, an ALD cobalt source and its carrier gas, and the remaining balance carrier gas, and the first panel is divided into a plurality of A fan-shaped area, the fan-shaped area includes a plurality of through holes distributed in an array; the radiation center of the cobalt source delivery channel is set to be an opening toward a gas mixing area of the second panel, and one end of the cobalt source delivery channel is connected to the gas mixing area; the other end of the cobalt source delivery channel is connected to the other end opening of the ventilation pipeline; the second panel includes a plurality of spray holes arranged along the circumferential direction and the radial direction, and a substrate support frame is installed at one end of the second panel away from the first panel; when the spray assembly is installed in the inner cavity, the output ends of the CVD cobalt source and its carrier gas pipeline, the ALD cobalt source and its carrier gas pipeline, and the output ends of the remaining balanced carrier gas pipelines are correspondingly connected to one end opening of the ventilation pipeline;
[0017] In the method for preparing the metal cobalt film, the CVD reaction gas and its carrier gas and the ALD reaction gas and its carrier gas flow to the area between the first panel and the second panel through the through hole, and the CVD cobalt source and its carrier gas and the ALD cobalt source and its carrier gas converge in the gas mixing area, diffuse and mix with the CVD reaction gas and its carrier gas and the ALD reaction gas and its carrier gas in the area between the first panel and the second panel, and then flow to the substrate through the spray hole.
[0018] In one embodiment of the present application, the diameter of the spray hole is smaller than the diameter of the through hole.
[0019] In a second aspect, the present application provides a metal cobalt film prepared by any of the methods described above.
[0020] In a third aspect, the present application provides a composite film comprising the metal cobalt thin film, including a composite substrate and a thin film layer, the thin film layer is a metal cobalt thin film, the composite substrate includes a substrate layer and an isolation layer attached to the substrate layer, and a thin film layer is formed by coating on the isolation layer.
[0021] The material of the substrate layer may be selected from silicon, silicon on insulator (SOI), quartz, sapphire or silicon carbide.
[0022] In one embodiment of the present application, the material of the substrate layer is silicon.
[0023] In the present application, the thickness of the substrate layer is not limited and can be specifically selected according to the product structure and the size of the substrate used.
[0024] In one embodiment of the present application, the material of the isolation layer may be selected from silicon dioxide, silicon oxynitride or silicon nitride.
[0025] In one embodiment of the present application, the material of the isolation layer is silicon dioxide.
[0026] Compared with the prior art, the beneficial effects of this application are:
[0027] The present application provides a metal cobalt film and a preparation method thereof. By combining the CVD method and the ALD method, in the preparation process of the metal cobalt film, the growth time of the obtained Co film is shorter (compared with ALD), the uniformity of growth within the film (film thickness) is better (compared with CVD) and the film resistivity is lower (compared with CVD). At the same time, the present application provides a spray assembly, which compresses the reduction reaction space of H2 and CCTBA to the local area between the first panel and the second panel, so that H2 can fully reduce CCTBA in a smaller space, and directly replace the 0-valent Co in the H2 atmosphere, reducing the influence of the non-uniformity of the reaction area and the gas phase diffusion effect on the deposition uniformity, and this design can effectively improve the uniformity of the pressure field above the substrate, and the uniform pressure helps to uniformly flow the mixed gas to the substrate surface through the spray hole of the second panel, avoiding the uneven deposition caused by excessive pressure gradient, and improving the uniformity of the film thickness of the deposited film. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a schematic diagram of the structure of the deposition equipment of this application;
[0029] Figure 2 An enlarged view of the top structure A of the deposition device of the present application;
[0030] Figure 3 This is a schematic diagram of the upper surface structure of the spray assembly of the present application;
[0031] Figure 4 This is a schematic diagram of the internal structure of the spray assembly of the present application;
[0032] Figure 5 This is a schematic diagram of the lower surface structure of the spray assembly of this application;
[0033] Figure 6 This is a schematic diagram of the installation position of the spray assembly in the inner cavity of the deposition equipment of this application;
[0034] Description of reference numerals:
[0035] A-top structure, 1-external cavity, 2-inner cavity, 3-plasma generator, 4-CVD reaction gas and its carrier gas pipeline, 5-inert gas pipeline, 6-ALD reaction gas and its carrier gas pipeline, 7-balanced carrier gas pipeline, 8-substrate transmission channel, 9-substrate support frame, 10-gas outlet, 100-first panel, 200-second panel, 300-cobalt source delivery channel, 400-gas mixing area, 110-fan-shaped area, 111-through hole, 210-spray hole, 500-columnar sidewall, 600-ventilation pipeline. DETAILED DESCRIPTION
[0036] The following will provide a clear and complete description of the technical solutions in the embodiments of the present application in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments.
[0037] The "range" disclosed in this application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range.
[0038] It should be noted that, in the description of the present application, “first” and “second” cannot be understood as indicating or implying relative importance, unless otherwise clearly specified and limited.
[0039] This application specification Figure 1-Figure 2 A cross-sectional view of the deposition equipment used in the present application and an enlarged schematic diagram of its top structure A are shown. The deposition equipment used in the present application mainly includes a closed outer cavity 1 and an inner cavity 2 arranged inside the outer cavity. A plasma generator 3 is arranged above the outer cavity 1. The output end of the plasma generator 3 is connected to the inlet of the inner cavity 2. The input end of the plasma generator 3 is connected to one or more CVD reaction gases and their carrier gas pipelines 4, one or more inert gas pipelines 5 and one or more ALD reaction gases and their carrier gas pipelines. In this embodiment, one CVD reaction gas and its carrier gas pipeline 4, one inert gas pipeline 5 and one ALD reaction gas and its carrier gas pipeline 6 are respectively arranged. The inner cavity includes an upper part 21 and a lower part 22 connected to each other, wherein the upper part 21 is a cone-shaped with a small top and a large bottom, and the lower part 22 is a basin-shaped, and the junction of the upper part 21 and the lower part 22 is the middle part of the circular inner cavity, and two or more balanced carrier gas pipelines are dispersed along the outer edge of the middle part of the inner cavity. In this embodiment, six balanced carrier gas pipelines 7 are arranged, and the six balanced carrier gas pipelines 7 are installed between the outer cavity 1 and the inner cavity 2 and the output ends are connected to the middle part of the inner cavity. It should be noted that the output ends of the six balanced carrier gas pipelines 7 connected to the middle part of the inner cavity are arranged opposite to each other. Each balanced carrier gas pipeline 7 can be connected to a cobalt source. When the cobalt source is connected, the balanced carrier gas pipeline 7 is used as a CVD or ALD cobalt source and its carrier gas pipeline. At this time, the balanced carrier gas is used as a carrier gas for the CVD cobalt source or the ALD cobalt source. A substrate transfer channel 8 is provided on the left side of the outer cavity 1. The left end of the substrate transfer channel 8 is a valve, which is connected to the vacuum transfer chamber. The right end of the substrate transfer channel 8 is connected to the inner cavity 2. A substrate support frame 9 is also provided inside the inner cavity 2, which is detachably connected to the wall of the inner cavity. An air outlet 10 is provided at the bottom of the inner cavity, and the air outlet 10 is externally connected to a vacuum pump for adjusting the pressure in the cavity.
[0040] It should be noted that the output port diameters of all pipelines in the inner cavity 2, including the CVD reaction gas and its carrier gas pipeline 4, the ALD reaction gas and its carrier gas pipeline 6, the inert gas pipeline 5, the CVD cobalt source and its carrier gas pipeline, the ALD cobalt source and its carrier gas pipeline, and the remaining balance carrier gas pipeline 7 except the CVD cobalt source and its carrier gas pipeline and the ALD cobalt source and its carrier gas pipeline, are the same.
[0041] The present application also designs a spray assembly, such as Figure 3-Figure 5 As shown, the spray assembly includes a columnar side wall 500 and a first panel 100 and a second panel 200 connected to both ends of the columnar side wall 500. The columnar side wall 500 has a thickness. Two or more ventilation pipes 600 are dispersedly arranged in the columnar side wall 500. In this embodiment, six ventilation pipes 600 are arranged. One end opening of the ventilation pipe 600 is located at the end of the columnar side wall 500 close to the second panel 200. The end of the columnar side wall 500 close to the first panel 100 is provided with a radial cobalt source delivery channel 300. The cobalt source delivery channel 300 is used to pass the CVD cobalt source and its carrier gas, the ALD cobalt source and its carrier gas, and the remaining flat The first panel 100 is divided into a plurality of fan-shaped areas 110 by a cobalt source delivery channel 300, and the fan-shaped area 110 includes a plurality of through holes 111 distributed in an array; the radiation center of the cobalt source delivery channel 300 is set to be an opening toward the gas mixing area 400 of the second panel, and one end of the cobalt source delivery channel 300 is connected to the gas mixing area 400; the other end of the cobalt source delivery channel 300 is connected to the other end of the ventilation pipeline 600; the second panel 200 includes a plurality of spray holes 210 arranged in the circumferential direction and the radial direction, and a substrate support frame is installed at the end of the second panel 200 away from the first panel 100;
[0042] like Figure 6 As shown, when the spray assembly is installed in the inner cavity, the output ends of the CVD cobalt source and its carrier gas pipeline, the ALD cobalt source and its carrier gas pipeline, and the remaining balanced carrier gas pipelines 7 except the CVD cobalt source and its carrier gas pipeline and the ALD cobalt source and its carrier gas pipeline are correspondingly connected to one end opening of the ventilation pipeline 600; the output port diameters of the CVD cobalt source and its carrier gas pipeline, the ALD cobalt source and its carrier gas pipeline, and the remaining balanced carrier gas pipelines 7 except the CVD cobalt source and its carrier gas pipeline and the ALD cobalt source and its carrier gas pipeline are consistent with the diameters of the cobalt source delivery channel 300 and the ventilation pipeline 600.
[0043] The method of using the deposition equipment in this application is as follows:
[0044] First, the inner cavity 2 is heated to the deposition temperature and then evacuated. Then, the substrate is delivered to the inner cavity 2 through the substrate transfer channel 8 to preheat the substrate. Then, the inert gas pipeline 5 and the plasma generator 3 are opened at the same time to pretreat the surface of the substrate to reduce the oxygen content and impurity particles on the surface of the substrate. After the pretreatment, the plasma generator 3 and the inert gas pipeline 5 are closed.
[0045] Subsequently, if a metal cobalt film is prepared by CVD, the plasma generator 3, six balanced carrier gas pipelines 7, CVD reaction gas and its carrier gas pipeline 4 are turned on at the same time, and the carrier gas flow rates of the six balanced carrier gas pipelines 7 are equal. Select any balanced carrier gas pipeline 7 to connect to the cobalt source as the CVD cobalt source and its carrier gas pipeline. After the reaction gas reacts with the cobalt source, it continues to deposit on the surface of the substrate to form a metal cobalt film. After the deposition is completed, all gas pipelines and plasma generators are closed, and the substrate is annealed. During the preparation process, the vacuum pump can discharge the excess cobalt source, CVD reaction gas and reaction by-products in the process reaction.
[0046] If a metal cobalt film is prepared by ALD, the plasma generator 3, six balanced carrier gas pipelines 7, ALD reaction gas and its carrier gas pipeline 6 (only the carrier gas of ALD reaction gas) are turned on at the same time, and the carrier gas flow rates of the six balanced carrier gas pipelines 7 are equal. The ALD method requires repeated multiple ALD cycles to complete the preparation of the metal cobalt film. Each ALD cycle includes four parts: ALD cobalt source pulse, ALD cobalt source carrier gas purge, ALD reaction gas pulse, and ALD reaction gas carrier gas purge. The specific details of the ALD cycle are: select a balanced carrier gas pipeline 7 to connect to the cobalt source and continue for a period of time before turning off the cobalt source (ALD cobalt source pulse), wait for a period of time (ALD cobalt source carrier gas purge), then turn on the ALD reaction gas and maintain it for a period of time before turning it off (ALD reaction gas pulse, at this time the cobalt source molecules on the substrate surface react with the reaction gas to form metal cobalt), then wait for a period of time (ALD reaction gas carrier gas purge), and then start the next ALD cycle. During the entire ALD process of preparing the metal cobalt film, the carrier gas flow in the balanced carrier gas pipeline 7 remains unchanged, the carrier gas flow of the ALD reaction gas remains unchanged, and the plasma generator 3 is always in the on state. During the preparation process, the vacuum pump can discharge the excess cobalt source, ALD reaction gas and reaction by-products in the process reaction. After the deposition is completed, all gas pipelines and plasma generators are closed, that is, the preparation process is terminated, and then the substrate is annealed.
[0047] If a metal cobalt film is prepared by combining CVD with ALD, the CVD and ALD processes start and end at the same time. First, the plasma generator 3, six horizontal carrier gas pipelines 7, CVD reaction gas and its carrier gas pipeline 4 (only CVD reaction gas carrier gas), ALD reaction gas and its carrier gas pipeline 6 (only ALD reaction gas carrier gas) are turned on at the same time, and then a balanced carrier gas pipeline 7 is selected as the CVD cobalt source and its carrier gas pipeline. The CVD process starts when the cobalt source is connected. When the CVD process starts, it is necessary to select another balanced carrier gas pipeline 7 with an output end opposite to the CVD cobalt source and its carrier gas pipeline as the ALD cobalt source and its carrier gas pipeline to start the ALD cycle process. When the CVD process ends, the ALD cycle process also ends at the same time. During the entire preparation process, the CVD reaction gas and its carrier gas pipeline 4, the ALD reaction gas and its carrier gas pipeline 6, the plasma generator 3, the CVD cobalt source and its carrier gas pipeline, the ALD cobalt source and its carrier gas pipeline, and the remaining balance carrier gas pipelines 7 are kept in an open state. At the same time, the ALD cobalt source and its carrier gas pipeline and the ALD reaction gas and its carrier gas pipeline 6 are opened or closed according to the needs of the ALD cycle. That is, the CVD reaction gas and its carrier gas, the carrier gas of the ALD reaction gas, the plasma generator, the CVD cobalt source and its carrier gas, the carrier gas of the ALD cobalt source, and the remaining balance carrier gas are kept in an open state, and the ALD cobalt source and the ALD reaction gas are opened or closed according to the needs of the ALD cycle. During the preparation process, the vacuum pump can discharge the excess cobalt source, CVD and ALD reaction gases and reaction by-products in the process reaction. Closing all gas pipelines and plasma generators means that the preparation process is terminated, and then the substrate is annealed.
[0048] The deposition device of the present application can use the above three methods to prepare metal cobalt thin films when a spray component is set or not set in the inner cavity.
[0049] The spray assembly provided in the present application has the following functions: the cobalt source and its carrier gas are converged in a small range within the gas mixing area 400 and then diffused to the surroundings, and the CVD reaction gas or ALD reaction gas rectified by the through hole 111 of the first panel 100 is fully mixed and reacted in the space between the first panel and the second panel, and then evenly dispersed by the spray hole of the second panel 200 and diffused downward to the substrate surface, reducing the non-uniformity of the reaction area and reducing the influence of the gas phase diffusion effect on the deposition uniformity. Moreover, this design can effectively improve the uniformity of the pressure field above the substrate, and the uniform pressure helps to evenly flow the mixed gas to the substrate surface through the spray hole of the second panel, avoiding the uneven deposition caused by the pressure gradient and improving the uniformity of the film thickness of the deposited film.
[0050] The deposition equipment of the above structure is used in the following embodiments of the present application, CCTBA is used as the CVD cobalt source and ALD cobalt source, H2 is used as the CVD reaction gas and ALD reaction gas, Ar is used as the carrier gas of the CVD reaction gas and ALD reaction gas, the remaining balance carrier gas and inert gas are used, and a metal cobalt film is prepared on a Si substrate or a Si composite substrate. Unless otherwise specified, the Si substrate or Si composite substrate used in the present application is circular.
[0051] The formula used in the embodiments of the present application is as follows:
[0052] (1) Inhomogeneity
[0053] First, calculate the standard deviation s (stdev) according to the following formula:
[0054] s 2 =[(x1-x)^2+(x2-x)^2+……(x n -x)^2] / n, x is the average film thickness (THK), there are n samples, x i is the film thickness at a single point;
[0055] Then, the non-uniformity 1-sigma value can be calculated from the standard deviation s and the average film thickness x(average(nm), that is:
[0056] 1-sigma = s / x*100%
[0057] (2) Resistivity ρ (μΩ·cm)
[0058] ρ=R*x / 10, R is the square resistance (Ω / □), and x is the average film thickness (average (nm)).
[0059] Example 1: Preparation of metal cobalt thin film by CVD method
[0060] This embodiment uses a deposition device without a spray assembly in the inner cavity, and the method steps for preparing a metal cobalt thin film include:
[0061] 1. The inner cavity is heated to the deposition temperature and then evacuated. The deposition temperature is preferably 100°C to 200°C, and in this embodiment it is 160°C. The pressure of the inner cavity is 1 torr, which is used to pretreat the substrate surface and reduce the oxygen content on the substrate surface.
[0062] 2. Place the substrate in a vacuum transfer chamber, and then evacuate the chamber. The pressure of the vacuum transfer chamber is preferably 0-2 torr, and is 1 torr in this embodiment. Perform Ar cyclic purge on the vacuum transfer chamber. During the cyclic purge, the pressure of the vacuum transfer chamber is 5 torr-300 torr, the Ar flow rate is 2000 sccm, and the number of cyclic purges is preferably 10-20 times, and is 10 times in this embodiment. After the cyclic purge, the pressure of the vacuum transfer chamber is preferably 0-2 torr, and is 1 torr in this embodiment. The purpose of the cyclic purge is to purge the impurity gases in the vacuum transfer chamber and on the surface of the substrate.
[0063] 3. Transfer the substrate from the vacuum transfer chamber to the inner chamber. During the transfer process, the pressure difference between the vacuum transfer chamber and the inner chamber does not exceed 1 torr. After the transfer is completed, close the vacuum transfer chamber, that is, close the outer chamber; heat the substrate to the deposition temperature and keep the temperature stable;
[0064] 4. Perform Ar plasma pretreatment on the substrate surface to reduce the oxygen content and impurity particles on the substrate surface. During the pretreatment, the plasma generator and Ar gas are turned on at the same time. The power of the plasma generator is 1000W, the Ar gas flow rate is 300sccm, the pretreatment time is 5min-10min, and the example is 5min. The pressure of the inner cavity is unlimited. After the pretreatment, the plasma generator and Ar gas are turned off;
[0065] 5. The deposition was carried out by CVD for 90 seconds. During the deposition by CVD, the plasma generator and H2 were turned on at the same time. The carrier gas Ar of H2 remained unchanged during the CVD process, and the flow rate was 1000 sccm. The plasma generator was continuously turned on during the CVD process, and the power of the plasma generator was 1000 W. The flow rate of H2 remained unchanged during the CVD process, and was 5000 sccm. The flow rate of the carrier gas Ar of the CVD cobalt source remained unchanged during the CVD process, and the flow rate was 500 sccm. The flow rate of the CVD cobalt source was 20 sccm, and remained unchanged during the CVD process. Except for the carrier gas Ar of the CVD cobalt source, the remaining balance carrier gas Ar was continuously turned on during the CVD process, and the balance carrier gas Ar flow rate was 500 sccm. The source temperature remained unchanged during the CVD process, and the source temperature was 45°C. The pressure of the inner cavity remained unchanged during the CVD process, and the pressure of the inner cavity was 10 torr.
[0066] 6. After the deposition reaction, the substrate in the inner cavity is annealed. The temperature of the inner cavity is preferably 100° C.-200° C., and in this embodiment it is 160° C. The annealing time is preferably 20-30 min, and in this embodiment it is 20 min.
[0067] 7. Transfer the substrate from the inner cavity to the vacuum transfer chamber and take it out.
[0068] The nine-point test results of the thickness (THK), square resistance, and resistivity of the cobalt film produced by the method of this embodiment using a 12-inch Si substrate are shown in Table 1 below:
[0069] Table 1 Test results of cobalt thin films on Si substrates prepared by CVD
[0070]
[0071] Note: In the table, (x, y) is the coordinate of the test point on the substrate, where the coordinate of the center of the substrate is (0, 0).
[0072] The nine-point test results of the thickness (THK), square resistance, and resistivity of the cobalt film made by the method of this embodiment using a 12-inch Si / 50nm SiO2 composite substrate are shown in Table 2 below:
[0073] Table 2 Test results of cobalt thin films on Si / 50nm SiO2 composite substrates prepared by CVD
[0074]
[0075] Note: In the table, (x, y) is the coordinate of the test point on the substrate, where the coordinate of the center of the substrate is (0, 0).
[0076] The nine-point test results of the thickness (THK), square resistance, and resistivity of the cobalt film made by the method of this embodiment using a 12-inch Si / 100nm SiO2 composite substrate are shown in Table 3 below:
[0077] Table 3 Test results of cobalt thin films on Si / 100nm SiO2 composite substrates prepared by CVD
[0078]
[0079] Note: In the table, (x, y) is the coordinate of the test point on the substrate, where the coordinate of the center of the substrate is (0, 0).
[0080] Example 2: Preparation of metal cobalt thin film by ALD method
[0081] This embodiment uses a deposition device without a spray assembly in the inner cavity, and the method steps for preparing a metal cobalt thin film include:
[0082] 1. The inner cavity is heated to the deposition temperature and then evacuated. The deposition temperature is preferably 100°C to 200°C, and in this embodiment it is 160°C. The pressure of the inner cavity is 1 torr, which is used to pretreat the substrate surface and reduce the oxygen content on the substrate surface.
[0083] 2. Place the substrate in a vacuum transfer chamber, and then evacuate the chamber. The pressure of the vacuum transfer chamber is preferably 0-2 torr, and is 1 torr in this embodiment. Perform Ar cyclic purge on the vacuum transfer chamber. During the cyclic purge, the pressure of the vacuum transfer chamber is 5 torr-300 torr, the Ar flow rate is 2000 sccm, and the number of cyclic purges is preferably 10-20 times, and is 10 times in this embodiment. After the cyclic purge, the pressure of the vacuum transfer chamber is preferably 0-2 torr, and is 1 torr in this embodiment. The purpose of the cyclic purge is to purge the impurity gases in the vacuum transfer chamber and on the surface of the substrate.
[0084] 3. Transfer the substrate from the vacuum transfer chamber to the inner chamber. During the transfer process, the pressure difference between the vacuum transfer chamber and the inner chamber does not exceed 1 torr. After the transfer is completed, close the vacuum transfer chamber, that is, close the outer chamber; heat the substrate to the deposition temperature and keep the temperature stable;
[0085] 4. Perform Ar plasma pretreatment on the substrate surface to reduce the oxygen content and impurity particles on the substrate surface. During the pretreatment, the plasma generator and Ar gas are turned on at the same time. The power of the plasma generator is 1000W, the Ar gas flow rate is 300sccm, the pretreatment time is 5min-10min, and the example is 5min. The pressure of the inner cavity is unlimited. After the pretreatment, the plasma generator and Ar gas are turned off;
[0086] 5. ALD was used for deposition for 90 seconds, and 6 cycles were used for deposition, with one cycle being 15 seconds (the pulse time of the ALD cobalt source was 1 second, the carrier gas purge time of the ALD cobalt source was 4 seconds, the pulse time of the ALD reaction gas was 3 seconds, and the carrier gas purge time of the ALD reaction gas was 7 seconds), totaling 90 seconds. The carrier gas Ar of H2 remained unchanged during the ALD process, with a flow rate of 1000 sccm. The power of the plasma generator was 1000 W. The flow rate of H2 remained unchanged during the ALD process, which was 5000 sccm. The flow rate of the ALD cobalt source carrier gas Ar remained unchanged during the ALD process, with a flow rate of 500 sccm. The flow rate of the ALD cobalt source was 20 sccm, which remained unchanged during the ALD process. Except for the carrier gas Ar of the ALD cobalt source, the remaining balance carrier gas Ar was continuously turned on during the ALD process, with a balance carrier gas Ar flow rate of 500 sccm. The source temperature remained unchanged during the ALD process, which was 45°C. The pressure of the inner cavity remained unchanged during the ALD process, which was 10 torr.
[0087] 6. After the deposition reaction, the substrate in the inner cavity is annealed. The temperature of the inner cavity is preferably 100° C.-200° C., and in this embodiment it is 160° C. The annealing time is preferably 20-30 min, and in this embodiment it is 20 min.
[0088] 7. Transfer the substrate from the inner cavity to the vacuum transfer chamber and take it out.
[0089] The nine-point test results of the thickness (THK), square resistance, and resistivity of the cobalt film produced by the method of this embodiment using a 12-inch Si substrate are shown in Table 4 below:
[0090] Table 4 Test results of cobalt thin films on Si substrates prepared by ALD
[0091]
[0092] Note: In the table, (x, y) is the coordinate of the test point on the substrate, where the coordinate of the center of the substrate is (0, 0).
[0093] The nine-point test results of the thickness (THK), square resistance, and resistivity of the cobalt film made by the method of this embodiment using a 12-inch Si / 50nm SiO2 composite substrate are shown in Table 5 below:
[0094] Table 5 Test results of cobalt thin films on Si / 50nm SiO2 composite substrates prepared by ALD
[0095]
[0096] Note: In the table, (x, y) is the coordinate of the test point on the substrate, where the coordinate of the center of the substrate is (0, 0).
[0097] The nine-point test results of the thickness (THK), square resistance, and resistivity of the cobalt film made by the method of this embodiment using a 12-inch Si / 100nm SiO2 composite substrate are shown in Table 6 below:
[0098] Table 6 Test results of cobalt thin films on Si / 100nm SiO2 composite substrates prepared by ALD
[0099]
[0100] Note: In the table, (x, y) is the coordinate of the test point on the substrate, where the coordinate of the center of the substrate is (0, 0).
[0101] Example 3: Preparation of Metal Cobalt Thin Film by Combining CVD and ALD
[0102] 1. The inner cavity is heated to the deposition temperature and then evacuated. The deposition temperature is preferably 100°C to 200°C, and in this embodiment it is 160°C. The pressure of the inner cavity is 1 torr, which is used to pretreat the substrate surface and reduce the oxygen content on the substrate surface.
[0103] 2. Place the substrate in a vacuum transfer chamber, and then evacuate the chamber. The pressure of the vacuum transfer chamber is preferably 0-2 torr, and is 1 torr in this embodiment. Perform Ar cyclic purge on the vacuum transfer chamber. During the cyclic purge, the pressure of the vacuum transfer chamber is 5 torr-300 torr, the Ar flow rate is 2000 sccm, and the number of cyclic purges is preferably 10-20 times, and is 10 times in this embodiment. After the cyclic purge, the pressure of the vacuum transfer chamber is preferably 0-2 torr, and is 1 torr in this embodiment. The purpose of the cyclic purge is to purge the impurity gases in the vacuum transfer chamber and on the surface of the substrate.
[0104] 3. Transfer the substrate from the vacuum transfer chamber to the inner chamber. During the transfer process, the pressure difference between the vacuum transfer chamber and the inner chamber does not exceed 1 torr. After the transfer is completed, close the vacuum transfer chamber, that is, close the outer chamber; heat the substrate to the deposition temperature and keep the temperature stable;
[0105] 4. Perform Ar plasma pretreatment on the substrate surface to reduce the oxygen content and impurity particles on the substrate surface. During the pretreatment, the plasma generator and Ar gas are turned on at the same time. The power of the plasma generator is 1000W, the Ar gas flow rate is 300sccm, the pretreatment time is 5min-10min, and the example is 5min. The pressure of the inner cavity is unlimited. After the pretreatment, the plasma generator and Ar gas are turned off;
[0106] 5. The deposition was performed by combining CVD with ALD for 90 s. The flow rates of the carrier gas Ar of the CVD reaction gas and the carrier gas Ar of the ALD reaction gas remained unchanged during the process, both at 1000 sccm. The plasma generator was continuously turned on during the CVD and ALD processes, and the power of the plasma generator was 1000 W. The flow rates of the CVD reaction gas H2 and the ALD reaction gas H2 remained unchanged during the process, both at 5000 sccm. The carrier gas of the CVD and ALD cobalt sources remained unchanged during the process, with a flow rate of 500 sccm. The flow rates of the CVD and ALD cobalt sources remained unchanged during the process, both at 20 sccm, the balance carrier gas Ar is continuously turned on during the CVD process, the balance carrier gas Ar flow rate except the CVD cobalt source carrier gas and the ALD cobalt source carrier gas Ar is 500sccm, the source temperature remains unchanged during the CVD and ALD processes, the source temperature is 45°C, the inner cavity pressure remains unchanged during the CVD and ALD processes, the inner cavity pressure is 10torr, CVD deposition is performed while ALD deposition is performed for 6 cycles, one cycle is 15s (ALD cobalt source pulse time is 1s, ALD cobalt source carrier gas purge time is 4s, ALD reaction gas pulse time is 3s, and ALD reaction gas carrier gas purge time is 7s);
[0107] 6. After the deposition reaction, the substrate in the inner cavity is annealed. The temperature of the inner cavity is preferably 100° C.-200° C., and in this embodiment it is 160° C. The annealing time is preferably 20-30 min, and in this embodiment it is 20 min.
[0108] 7. Transfer the substrate from the inner cavity to the vacuum transfer chamber and take it out.
[0109] Using the embodiment method, the nine-point test results of the thickness (THK), square resistance, and resistivity of the cobalt film made on a 12-inch Si substrate are shown in Table 7 below:
[0110] Table 7 Test results of cobalt thin films on Si substrates prepared by CVD-ALD
[0111]
[0112] Note: In the table, (x, y) is the coordinate of the test point on the substrate, where the coordinate of the center of the substrate is (0, 0).
[0113] The nine-point test results of the thickness (THK), square resistance, and resistivity of the cobalt film made by the method of this embodiment using a 12-inch Si / 50nm SiO2 composite substrate are shown in Table 8 below:
[0114] Table 8 Test results of cobalt thin films on Si / 50nm SiO2 composite substrates prepared by CVD-ALD
[0115]
[0116] Note: In the table, (x, y) is the coordinate of the test point on the substrate, where the coordinate of the center of the substrate is (0, 0).
[0117] The nine-point test results of the thickness (THK), square resistance, and resistivity of the cobalt film made by the method of this embodiment using a 12-inch Si / 100nm SiO2 composite substrate are shown in Table 9 below:
[0118] Table 9 Test results of cobalt thin films on Si / 100nm SiO2 composite substrates prepared by CVD-ALD
[0119]
[0120] Note: In the table, (x, y) is the coordinate of the test point on the substrate, where the coordinate of the center of the substrate is (0, 0).
[0121] Example 4: After the spray assembly is set in the inner cavity, the metal cobalt film is prepared by CVD combined with ALD
[0122] This embodiment uses a deposition device with a spray assembly arranged in the inner cavity. The method steps for preparing the metal cobalt thin film are compared with those of Example 3, and the other experimental conditions are the same. The difference is that a spray assembly is arranged in the inner cavity of the deposition device, and the output ends of the six balanced carrier gas pipelines are correspondingly connected to the openings at one end of the ventilation pipeline 600. Any two relatively arranged balanced carrier gas pipelines are connected to the cobalt source, which are respectively used as the cobalt source and its carrier gas pipeline of CVD and the cobalt source and its carrier gas pipeline of ALD.
[0123] The nine-point test results of the thickness (THK), square resistance, and resistivity of the cobalt film produced by the method of this embodiment using a 12-inch Si substrate are shown in Table 10 below:
[0124] Table 10 Test results of cobalt thin films on Si substrates prepared by spray assembly + CVD-ALD
[0125]
[0126] Note: In the table, (x, y) is the coordinate of the test point on the substrate, where the coordinate of the center of the substrate is (0, 0).
[0127] Using the method of this embodiment, the nine-point test results of the thickness (THK), square resistance, and resistivity of the cobalt film made on a 12-inch Si / 50nm SiO2 composite substrate are shown in Table 11 below:
[0128] Table 11 Test results of cobalt thin films on Si / 50nm SiO2 composite substrates prepared by spray assembly + CVD-ALD
[0129]
[0130] Note: In the table, (x, y) is the coordinate of the test point on the substrate, where the coordinate of the center of the substrate is (0, 0).
[0131] The nine-point test results of the thickness (THK), square resistance, and resistivity of the cobalt film made by the method of this embodiment using a 12-inch Si / 100nm SiO2 composite substrate are shown in Table 12 below:
[0132] Table 12 Test results of cobalt thin films on Si / 100nm SiO2 composite substrates prepared by spray assembly + CVD-ALD
[0133]
[0134] Note: In the table, (x, y) is the coordinate of the test point on the substrate, where the coordinate of the center of the substrate is (0, 0).
[0135] The test results of different cobalt films obtained in Examples 1-4 are analyzed as follows:
[0136] (1) After calculating the uniformity of the thickness at nine test points of the cobalt films prepared in Example 1 and Example 3, as shown in Table 13, the non-uniformity of the cobalt films prepared on three different substrates by the CVD combined with ALD method was greatly reduced by 50%-62% compared with the CVD preparation method alone, indicating that the CVD combined with ALD preparation method can effectively improve the uniformity of the cobalt film.
[0137] Table 13 1-sigma (%)-uniformity comparison of cobalt thin films
[0138]
[0139] (2) The average resistivity of the nine test points of the cobalt thin films prepared in Example 1 and Example 3 were compared, as shown in Table 14. Compared with the cobalt thin film prepared by CVD combined with ALD, the cobalt thin film prepared by CVD alone can significantly reduce the resistivity of the prepared cobalt thin film, making the performance of the cobalt thin film better.
[0140] Table 14 Comparison of cobalt film resistivity (μΩ·cm)
[0141]
[0142] (3) After calculating the growth time and average film thickness of the cobalt thin films obtained in Example 2 and Example 3, the growth rate was obtained and compared. As shown in Table 15, the growth rate of the cobalt thin film prepared by the CVD combined with ALD method was significantly increased by about 25 times compared with the single ALD method.
[0143] Table 15 Comparison of cobalt film growth rate (Å / min)
[0144]
[0145] (4) After calculating the uniformity of the thickness at nine test points of the cobalt thin films obtained in Example 3 and Example 4, as shown in Table 16, the non-uniformity of the cobalt thin films was further significantly reduced by more than 50% using the CVD combined with ALD method using a spray component and the CVD combined with ALD method without a spray component, indicating that the use of a spray component can effectively improve the uniformity of the cobalt thin film.
[0146] Table 16 1-sigma (%)-uniformity comparison of CVD-ALD method with spray assembly and without spray assembly
[0147]
[0148] (5) The average resistivity of the cobalt films at nine test points obtained in Example 3 and Example 4 was compared, as shown in Table 17. The resistivity of the cobalt films was significantly reduced when the CVD combined with ALD method using a spray component was used and when the CVD combined with ALD method not using a spray component was used, indicating that the use of a spray component can also effectively reduce the resistivity of the cobalt film.
[0149] Table 17 Comparison of resistivity (μΩ·cm) of CVD-ALD with and without spray assembly
[0150]
[0151] The relevant performance test data of the cobalt thin films prepared in the above embodiments of the present application and the embodiments show that the present invention combines the CVD method and the ALD method to prepare the cobalt thin film, and has a higher growth efficiency than the cobalt thin film prepared by the ALD method, and has better growth uniformity (film thickness) within the cobalt thin film sheet and lower film resistivity than the cobalt thin film prepared by the CVD method. At the same time, the present application provides a spray assembly of a deposition device, which compresses the reduction reaction space of H2 and CCTBA to the local area of the first panel and the second panel, reduces the influence of the non-uniformity of the reaction area and the gas phase diffusion effect on the deposition uniformity, and further improves the film thickness uniformity of the cobalt thin film and reduces the resistivity on the basis of combining the CVD method with the ALD method.
Claims
1. A method for preparing a metal cobalt thin film, characterized in that: include: The method is applied to an inner cavity of a deposition device, wherein a substrate is placed in the inner cavity, and the method uses CVD and ALD to simultaneously react a cobalt source and a reaction gas to deposit a metal cobalt film on the substrate; The deposition device is provided with 2 or more balanced carrier gas pipelines passing into the inner cavity, 1 or more CVD reaction gas and its carrier gas pipeline, and 1 or more ALD reaction gas and its carrier gas pipeline passing into the inner cavity through a plasma generator. When the balanced carrier gas pipeline is connected to the cobalt source, it is used as a CVD cobalt source and its carrier gas pipeline or an ALD cobalt source and its carrier gas pipeline. At this time, the balanced carrier gas is used as a carrier gas for the CVD cobalt source or the ALD cobalt source; In the method, the CVD reaction gas and its carrier gas pipeline, the ALD reaction gas and its carrier gas pipeline, the plasma generator, the CVD cobalt source and its carrier gas pipeline, the ALD cobalt source and its carrier gas pipeline, and the remaining balanced carrier gas pipelines except the CVD cobalt source and its carrier gas pipeline and the ALD cobalt source and its carrier gas pipeline are always kept in an open state. At the same time, the ALD cobalt source and its carrier gas pipeline and the ALD reaction gas and its carrier gas pipeline are opened or closed according to the needs of the ALD cycle. The ALD cycle includes: ALD cobalt source pulse, ALD cobalt source carrier gas purge, ALD reaction gas pulse, and ALD reaction gas carrier gas purge; The deposition device is also provided with an inert gas pipeline passing through the plasma generator into the inner cavity, and the output port diameters of the inert gas pipeline, the CVD reaction gas and its carrier gas pipeline, the ALD reaction gas and its carrier gas pipeline, the CVD cobalt source and its carrier gas pipeline, the ALD cobalt source and its carrier gas pipeline, and the remaining balance carrier gas pipelines are all the same; under this condition, the gas flow rates of the carrier gas of the CVD cobalt source and the ALD cobalt source and the remaining balance carrier gas are equal, the flow rates of the CVD cobalt source and the ALD cobalt source are equal, the carrier gas flow rates of the CVD reaction gas and the ALD reaction gas are equal, and the flow rates of the CVD reaction gas and the ALD reaction gas are equal; A detachable spray assembly is arranged in the inner cavity of the deposition device, and the spray assembly comprises a columnar side wall (500) and a first panel (100) and a second panel (200) connected to both ends of the columnar side wall (500). The columnar side wall (500) has a thickness. Two or more ventilation pipes (600) are dispersedly arranged in the columnar side wall (500). One end opening of the ventilation pipe (600) is located at an end of the columnar side wall (500) close to the second panel (200). A radial cobalt source delivery channel (300) is arranged at an end of the columnar side wall (500) close to the first panel (100). The cobalt source delivery channel (300) is used to introduce a CVD cobalt source and its carrier gas, an ALD cobalt source and its carrier gas, and the remaining balance carrier gas. The first panel (100) is divided into a plurality of fan-shaped areas (110) by a cobalt source delivery channel (300), and the fan-shaped area (110) includes a plurality of through holes (111) distributed in an array; the radiation center of the cobalt source delivery channel (300) is set to open toward the gas mixing area (400) of the second panel, and one end of the cobalt source delivery channel (300) is connected to the gas mixing area (400); the other end of the cobalt source delivery channel (300) is connected to the other end opening of the ventilation pipeline (600); the second panel (200) includes a plurality of spray holes (210) arranged in a circumferential direction and a radial direction, and a substrate support frame is installed at one end of the second panel (200) away from the first panel (100); when the spray assembly is installed in the inner cavity, the output ends of the CVD cobalt source and its carrier gas pipeline, the ALD cobalt source and its carrier gas pipeline, and the output ends of the remaining balanced carrier gas pipelines are correspondingly connected to one end opening of the ventilation pipeline (600); In the method for preparing the metal cobalt thin film, the CVD reaction gas and its carrier gas and the ALD reaction gas and its carrier gas flow to the area between the first panel (100) and the second panel (200) through the through hole (111); the CVD cobalt source and its carrier gas and the ALD cobalt source and its carrier gas converge in the gas mixing area (400), diffuse and mix with the CVD reaction gas and its carrier gas and the ALD reaction gas and its carrier gas in the area between the first panel (100) and the second panel (200), and then flow to the substrate through the spray hole (210).
2. The method for preparing a metal cobalt thin film according to claim 1, characterized in that: The inert gas pipeline is used for plasma pretreatment of the substrate surface.
3. The method for preparing a metal cobalt thin film according to claim 1, characterized in that: The preparation method also includes annealing the metal cobalt film.
4. The method for preparing a metal cobalt thin film according to claim 1, characterized in that: The CVD process and the ALD process are started and stopped simultaneously, and the number of ALD cycles for completing ALD deposition during the CVD period is no less than 1.
5. The method for preparing a metal cobalt thin film according to claim 1, characterized in that: The CVD cobalt source and the ALD cobalt source are CCTBA, the CVD reaction gas and the ALD reaction gas are H2, and the carrier gas of the CVD reaction gas and the ALD reaction gas, the remaining balance carrier gas and the inert gas are Ar.
6. The method for preparing a metal cobalt thin film according to claim 5, characterized in that: During the preparation of the metal cobalt film, the inner cavity deposition temperature is 100°C-200°C, and the cavity pressure of the inner cavity is 8torr-12torr during the CVD and ALD processes; the flow rates of the CVD reaction gas and the ALD reaction gas H2 are 5000sccm respectively, the flow rates of the carrier gas Ar of the CVD reaction gas and the ALD reaction gas are 1000sccm respectively, the flow rates of the CVD cobalt source and the ALD cobalt source CCTBA are 0-30sccm respectively, the flow rates of the carrier gas of the CVD cobalt source and the ALD cobalt source and the remaining balance carrier gas Ar are 500sccm respectively, the power of the plasma generator is 1000W, and the temperature of the cobalt source CCTBA is 45°C.
7. The method for preparing a metal cobalt thin film according to claim 6, characterized in that: The time for one cycle of the ALD is 15s, including: the ALD cobalt source pulse time is 1s, that is, the ALD cobalt source turn-on time is 1s; the carrier gas purge time of the ALD cobalt source is 4s, that is, the ALD cobalt source turn-off time is 4s; the ALD reaction gas pulse time is 3s, that is, the ALD reaction gas turn-on time is 3s; the ALD reaction gas carrier gas purge time is 7s, that is, the ALD reaction gas turn-off time is 7s.
8. The method for preparing a metal cobalt thin film according to claim 1, characterized in that: The diameter of the spray hole (210) is smaller than the diameter of the through hole (111).
9. The metal cobalt thin film prepared by the method according to any one of claims 1 to 8.
10. A composite film comprising the metal cobalt film according to claim 9, characterized in that: The composite film comprises a composite substrate and a film layer, wherein the film layer is a metal cobalt film; the composite substrate comprises a substrate layer and an isolation layer attached to the substrate layer; and a film is formed by coating the isolation layer.
Citation Information
Patent Citations
NMOS metal gate materials, manufacturing methods, and equipment using CVD and ALD processes with metal based precursors
CN102918636A
Method for growing CoSix film by using thermal atomic layer deposition technology ALD
CN112281138A
Process for pulsed thin film deposition
CN113661269A
Atomic layer deposition method of cobalt-based oxide film
CN114540793A