A normally-off high electron mobility transistor and a method for manufacturing the same

By injecting non-electroactive material ions into the barrier layer of the GaN HEMT device to form an insulator layer, the problem of electron mobility and Vth stability of the normally-off GaN HEMT device in the existing technology is solved, and high mobility and adjustable Vth, reducing packaging complexity and cost.

CN118380466BActive Publication Date: 2024-10-29JIANGSU CORENERGY SEMICON CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410830939.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-29
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

It is difficult to manufacture normally-off GaN HEMT devices with high electron mobility and adjustable threshold voltage (Vth) using existing technology, and there are problems such as complex packaging, high cost, and poor performance.

Method used

By injecting non-electroactive material ions, such as nitrogen ions or inert gas ions, into the barrier layer of the GaN HEMT device, an insulator layer is formed, thereby invalidating the naturally formed 2DEG layer and avoiding etching and damage to the barrier layer. Increased stability and adjustability of Vth.

Benefits of technology

It achieves high electron mobility and stable Vth, while avoiding mobility decrease and Vth instability caused by charge scattering, reducing packaging complexity and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118380466B_ABST
    Figure CN118380466B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of high electron mobility transistor devices, and specifically relates to a normally-off high electron mobility transistor and a method for preparing the same. In the normally-off high electron mobility transistor provided by the present invention, the barrier layer is injected with non-electrically active material ions, and the injection area of ​​the non-electrically active material ions coincides with the positive projection area of ​​the gate on the barrier layer, and the non-electrically active material ions include nitrogen ions and / or inert gas ions. The barrier layer and the channel layer of the present invention have a more stable Vth and an original unetched and undamaged 2DEG layer. The present invention converts the barrier layer into an insulator by injecting non-electrically active material ions into the barrier layer, thereby rendering the naturally formed 2DEG layer invalid. Compared with the introduction of electrically active elements (such as chlorine or fluorine atoms), the present invention does not have the defects of decreased mobility due to charge scattering and unstable Vth due to the movement of chlorine or fluorine ions under gate bias.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of high electron mobility transistor devices, and in particular relates to a normally-off high electron mobility transistor and a preparation method thereof. Background Art

[0002] GaN-based high electron mobility transistor (GaN HEMT) devices are normally-on (depletion mode, gate threshold voltage, Vth < 0V) devices. This is because a two-dimensional electron gas (2DEG) layer is naturally formed at the interface between the barrier layer (AlGaN, AlN, InAlN, etc.) and the channel layer (usually GaN) due to the physical effects of spontaneous polarization and piezoelectric polarization, such as AlGaN / GaN structure or AlN / GaN structure or InAlN / GaN structure. The structural schematic diagram of the normally-on GaN HEMT device is shown in Figure 1 However, in practical power switching applications, normally-off (enhancement mode, gate threshold voltage, Vth>0V) devices are required.

[0003] At present, the following methods reported in the prior art can manufacture normally-off GaN HEMT devices, some of which have been commercially verified and are in mass production, as shown below:

[0004] The first solution, the "two-chip" solution (commercially available), involves Figure 2 A normally-off Si MOSFET device and a normally-on GaN HEMT device in a cascade cathode (Cascode) configuration (“Cascode” device) shown, where the Vth of the combined device is only the Vth of the Si MOSFET device, ranges from 2 to 4 V and is available from many suppliers. However, the Cascode approach is a two-chip solution with complex packaging and requires careful matching of the two device parameters to work as a single unit, resulting in high costs.

[0005] The second solution (commercially available) is to add an in-situ grown Mg-doped p-type GaN layer on top of the barrier layer (e.g. AlGaN) to physically deplete the underlying 2DEG layer resulting in a tuned conduction band, e.g. Figure 3 The schematic diagram of the structure of the "p-GaN gate" device. The typical Vth is in the range of 1~2V. However, the device obtained by the method of in-situ growth of the Mg-doped p-type GaN layer has low gate breakdown (<10V) and a small gate drive voltage range of 5~6V, and the device performance is poor.

[0006] A third solution (not commercially available) is to completely remove the barrier layer such as AlGaN by dry plasma etching under the gate region, thereby eliminating the naturally formed 2DEG layer, and deposit a subsequent insulating layer such as SiO2, Al2O3, SiN, AlN or other high-k materials only under the gate region by plasma enhanced chemical vapor deposition (PECVD), low pressure chemical vapor deposition (LPCVD), atomic layer deposition (ALD), or a combination thereof to produce a metal insulator semiconductor gate structure, such as Figure 4 The conventional Si and SiC MOSFET devices shown are the same (“MIS gate” devices). Vth can be adjusted from 1V to 4V depending on the insulator thickness and its material properties. After the barrier layer is etched, the damaged and rough GaN channel surface causes the interface between the subsequently deposited dielectric layer and the GaN channel layer to have a high level of electrically active trap density, resulting in low interface electron mobility, low on-current and Vth instability.

[0007] A fourth solution (not commercially available) is to introduce strongly electronegative and electrically active elements (such as chlorine or fluorine atoms) into the barrier layer (such as AlGaN) by high-density plasma treatment or low-energy ion implantation, thereby expelling only the lower electrons in the 2DEG layer in the gate region, such as Figure 5 A "depleted gate" device is shown. The typical Vth has only a limited range, usually less than 1.0V. At the same time, negatively charged ions will deteriorate interface mobility and Vth stability is poor. Summary of the invention

[0008] The object of the present invention is to provide a normally-off high electron mobility transistor and a method for preparing the same. The normally-off high electron mobility transistor device provided by the present invention has high interface electron mobility, no excessive Coulomb scattering centers, and has an adjustable and more stable Vth.

[0009] In order to achieve the above object, the present invention provides the following technical solutions:

[0010] The present invention provides a normally-off high electron mobility transistor, comprising a substrate layer; a buffer layer arranged on the upper surface of the substrate layer; a channel layer arranged on the upper surface of the buffer layer; a source electrode arranged on part of the upper surface of the channel layer, a drain electrode arranged on part of the upper surface, and a barrier layer arranged on part of the upper surface; a gate electrode arranged on part of the upper surface of the barrier layer; the barrier layer is injected with non-electrically active material ions, the injection area of ​​the non-electrically active material ions in the barrier layer coincides with the positive projection area of ​​the gate electrode on the barrier layer, and the non-electrically active material ions include nitrogen ions and / or inert gas ions.

[0011] Preferably, the inert gas ions include Ar ions.

[0012] Preferably, the implantation density of the non-electroactive substance ions is 1E13-1E15 cm -2 ; The injection energy of the non-electroactive material ions is 10~100 keV.

[0013] Preferably, the method further comprises: a first insulating layer disposed between the barrier layer and the gate, wherein a projection area of ​​the first insulating layer on the upper surface of the barrier layer overlaps with a projection area of ​​the gate on the upper surface of the barrier layer.

[0014] Preferably, the material of the first insulating layer includes one or more of SiO2, Al2O3, SiN, AlN or other high dielectric constant dielectric materials, and the dielectric constant of the other high dielectric constant dielectric materials is greater than 9 F / m.

[0015] Preferably, the thickness of the first insulating layer is 0-100 nm, and is not 0 nm.

[0016] Preferably, the barrier layer comprises non-electrically active material ions and a host material, and the host material comprises one or more of AlGaN, AlN and InAlN;

[0017] The material of the channel layer is GaN.

[0018] The present invention provides a method for preparing a normally-off high electron mobility transistor according to the above technical solution, comprising the following steps:

[0019] Sequentially preparing a buffer layer and a channel layer on the upper surface of the substrate layer;

[0020] Preparing a source electrode, a drain electrode and an initial barrier layer on the upper surface of the channel layer;

[0021] Injecting non-electrically active material ions into the initial barrier layer to obtain a barrier layer; the injection region of the non-electrically active material ions into the initial barrier layer coincides with the positive projection region of the gate on the barrier layer;

[0022] A gate is prepared on the upper surface of the region of the barrier layer where the non-electrically active material ions are implanted.

[0023] Preferably, the implantation method includes plasma implantation or low-energy ion implantation.

[0024] Preferably, after obtaining the barrier layer and before preparing the gate, it also includes: preparing a first insulating layer on the upper surface of the region where the barrier layer is injected with non-electrically active material ions; after obtaining the first insulating layer, preparing the gate on the upper surface of the first insulating layer.

[0025] The present invention provides a normally-off high electron mobility transistor, comprising a substrate layer; a buffer layer arranged on the upper surface of the substrate layer; a channel layer arranged on the upper surface of the buffer layer; a source electrode arranged on part of the upper surface of the channel layer, a drain electrode arranged on part of the upper surface, and a barrier layer arranged on part of the upper surface; a gate electrode arranged on part of the upper surface of the barrier layer; the barrier layer is injected with non-electrically active material ions, the injection area of ​​the non-electrically active material ions in the barrier layer coincides with the positive projection area of ​​the gate electrode on the barrier layer, and the non-electrically active material ions include nitrogen ions and / or inert gas ions. Compared with the above-mentioned "third solution", the present invention does not etch or damage the barrier layer, and has a more stable Vth and an original unetched and undamaged 2DEG layer between the barrier layer and the channel layer. Compared with the above-mentioned "fourth solution", the present invention converts the barrier layer into an insulator by injecting non-electrically active material ions into the barrier layer, thereby rendering the naturally formed 2DEG layer ineffective. Compared with the introduction of electrically active elements (such as chlorine or fluorine atoms), the present invention does not have the defects of decreased mobility due to charge scattering and unstable Vth due to the movement of chlorine or fluorine ions under gate bias. In summary, the normally-off high electron mobility transistor device provided by the present invention has high interface electron mobility, no excessive Coulomb scattering centers, and has an adjustable and more stable Vth.

[0026] Furthermore, in the present invention, the inert gas ions include Ar ions. Ar ions have a relatively large atomic size and are therefore not easily distributed and extended into the GaN channel layer below the barrier layer, thereby ensuring that the normally-off high electron mobility transistor device has a more stable Vth.

[0027] Furthermore, in the present invention, the normally-off high electron mobility transistor further includes: a first insulating layer disposed between the barrier layer and the gate, wherein the projection area of ​​the first insulating layer on the upper surface of the barrier layer overlaps with the projection area of ​​the gate on the upper surface of the barrier layer. The first insulating layer can effectively reduce gate leakage current, increase gate breakdown voltage, and achieve an appropriate turn-on threshold voltage in Si MOSFET or SiC MOSFET. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of the structure of a normally-on GaN HEMT device in the prior art;

[0029] Figure 2 A diagram of a combination of Si MOSFET and normal-conducting GaN HEMT in a cascode configuration in the prior art;

[0030] Figure 3 It is a schematic diagram of the structure of a "p-GaN gate" device in the prior art;

[0031] Figure 4 A schematic diagram of the structure of a conventional Si MOSFET device and a SiC MOSFET device ("MIS gate" device) in the prior art;

[0032] Figure 5 It is a structural schematic diagram of an "enhancement gate" device in the prior art;

[0033] Figure 6 A schematic diagram of the structure of a normally-off high electron mobility transistor device provided by the present invention;

[0034] Figure 7 A schematic structural diagram of a normally-off high electron mobility transistor device having a first insulating layer provided by the present invention;

[0035] Among them: 1 is a substrate layer, 2 is a buffer layer, 3 is a channel layer, 4 is a barrier layer, 5 is a source, 6 is a drain, 7 is a gate, 8 is a 2DEG layer, 9 is a Mg-doped P-type GaN layer, 10 is a second insulating layer, 11 is an electrically active element injection layer, 12 is an electrically inactive element injection layer, and 13 is a first insulating layer. DETAILED DESCRIPTION

[0036] The present invention provides a normally-off high electron mobility transistor, comprising a substrate layer; a buffer layer arranged on the upper surface of the substrate layer; a channel layer arranged on the upper surface of the buffer layer; a source electrode arranged on part of the upper surface of the channel layer, a drain electrode arranged on part of the upper surface, and a barrier layer arranged on part of the upper surface; a gate electrode arranged on part of the upper surface of the barrier layer; the barrier layer is injected with non-electrically active material ions, the injection area of ​​the non-electrically active material ions in the barrier layer coincides with the positive projection area of ​​the gate electrode on the barrier layer, and the non-electrically active material ions include nitrogen ions and / or inert gas ions.

[0037] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.

[0038] Figure 6 The schematic diagram of the structure of the normally-off high electron mobility transistor device provided by the present invention is shown below. Figure 6 , the structure of the normally-off high electron mobility transistor device provided by the present invention is described in detail.

[0039] In the present invention, the normally-off high electron mobility transistor device is preferably a normally-off GaN HEMT device.

[0040] The normally-off high electron mobility transistor provided by the present invention comprises a substrate layer 1. In the present invention, the material of the substrate layer 1 is preferably Si, SiC or sapphire. The thickness of the substrate layer 1 is preferably less than 300 μm.

[0041] The normally-off high electron mobility transistor provided by the present invention comprises a buffer layer 2 arranged on the upper surface of the substrate layer. In the present invention, the material of the buffer layer 2 is AlGaN.

[0042] The normally-off high electron mobility transistor provided by the present invention comprises a channel layer 3 arranged on the upper surface of the buffer layer. In the present invention, the material of the channel layer 3 is preferably GaN.

[0043] The normally-off high electron mobility transistor provided by the present invention comprises a source 5 arranged on a portion of the upper surface of the channel layer, a drain 6 on a portion of the upper surface, and a barrier layer 4 on a portion of the upper surface. In the present invention, the source 5 and the drain 6 are conductive metal contact layers of the channel layer. The barrier layer 4 comprises non-electrically active material ions and a main material, and the main material preferably comprises one or more of AlGaN, AlN and InAlN, more preferably AlGaN. The non-electrically active material ions comprise nitrogen ions and / or inert gas ions. The inert gas ions preferably comprise Ar ions. The injection density of the non-electrically active material ions is preferably 1E13~1E15 cm -2 , more preferably 1E14 cm -2 The injection energy of the non-electroactive material ions is preferably 10-100 keV.

[0044] The normally-off high electron mobility transistor provided by the present invention comprises a gate 7 arranged on the upper surface of the barrier layer portion; the barrier layer 4 is injected with non-electrically active material ions, the injection area of ​​the non-electrically active material ions in the barrier layer 4 coincides with the positive projection area of ​​the gate 7 on the barrier layer 4, and the thickness of the injection area of ​​the non-electrically active material ions in the barrier layer 4 is equal to the thickness of the barrier layer 4. The non-electrically active material ions include nitrogen ions and / or inert gas ions.

[0045] Figure 7 A schematic diagram of the structure of a normally-off high electron mobility transistor device with a first insulating layer provided by the present invention is shown in FIG. Figure 7 As shown, the normally-off high electron mobility transistor provided by the present invention preferably further includes: a first insulating layer 13 disposed between the barrier layer and the gate, wherein the projection area of ​​the first insulating layer 13 on the upper surface of the barrier layer 4 overlaps with the projection area of ​​the gate 7 on the upper surface of the barrier layer 4. In the present invention, the material of the first insulating layer 13 preferably includes one or more of SiO2, Al2O3, SiN, AlN or other high-dielectric constant dielectric materials, and the dielectric constant of the other high-dielectric constant dielectric materials is preferably greater than 9 F / m. The thickness of the first insulating layer 13 is preferably 0~100nm, and is not 0nm, and more preferably 1~100nm.

[0046] The present invention provides a method for preparing a normally-off high electron mobility transistor according to the above technical solution, comprising the following steps:

[0047] Sequentially preparing a buffer layer and a channel layer on the upper surface of the substrate layer;

[0048] Preparing a source electrode, a drain electrode and an initial barrier layer on the upper surface of the channel layer;

[0049] Injecting non-electrically active material ions into the initial barrier layer to obtain a barrier layer; the injection region of the non-electrically active material ions into the initial barrier layer coincides with the positive projection region of the gate on the barrier layer;

[0050] A gate is prepared on the upper surface of the region of the barrier layer where the non-electrically active material ions are implanted.

[0051] The present invention sequentially prepares a buffer layer and a channel layer on the upper surface of the substrate layer. The present invention has no special requirements on the preparation methods of the buffer layer and the channel layer.

[0052] After obtaining the channel layer, the present invention prepares a source electrode, a drain electrode and an initial barrier layer on the upper surface of the channel layer. The present invention has no special requirements on the preparation method of the source electrode, the drain electrode and the initial barrier layer. The initial barrier layer preferably includes one or more of AlGaN, AlN and InAlN, and more preferably AlGaN.

[0053] After obtaining the initial barrier layer, the present invention injects non-electrically active material ions into the initial barrier layer to obtain the barrier layer; the injection area of ​​the non-electrically active material ions in the initial barrier layer coincides with the positive projection area of ​​the gate on the barrier layer. The injection density of the non-electrically active material ions is preferably 1E13~1E15 cm -2 , more preferably 1E14cm -2 . The injection energy of the non-electrically active material ions is preferably 10~100 keV. The injection method preferably includes plasma injection or low-energy ion injection. The injection time of the non-electrically active material ions is based on the injection density and injection energy (depth) of the non-electrically active material ions in the barrier layer to render the naturally formed 2DEG layer ineffective. The present invention has no special requirements for the specific implementation of ion injection. In a specific embodiment of the present invention, ion injection is performed by standard photolithography patterning.

[0054] After obtaining the barrier layer, the present invention prepares a gate on the upper surface of the region of the barrier layer where the non-electrically active material ions are injected. The present invention has no special requirements on the specific preparation method of the gate.

[0055] In the present invention, after obtaining the barrier layer and before preparing the gate, the present invention preferably further comprises: preparing a first insulating layer on the upper surface of the region where the non-electrically active material ions are injected into the barrier layer; after obtaining the first insulating layer, preparing the gate on the upper surface of the first insulating layer. The present invention has no special requirements for the preparation method of the first insulating layer.

[0056] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0057] Example 1

[0058] Preparation Figure 6 The normally-off GaN HEMT device of the structure shown in the figure has a specific preparation method comprising the following steps:

[0059] An AlGaN buffer layer and a GaN channel layer are prepared on the upper surface of a substrate layer (thickness is ~1 mm) made of Si, SiC or sapphire.

[0060] An AlGaN initial barrier layer, a source electrode and a drain electrode are prepared on the upper surface of the GaN channel layer.

[0061] The barrier layer is obtained by injecting Ar ions into the AlGaN initial barrier layer, wherein the injection area of ​​the Ar ions in the AlGaN initial barrier layer coincides with the area of ​​the positive projection of the gate on the barrier layer. The injection energy of the Ar ions is 10-100 keV; the injection method includes plasma injection or low-energy ion injection, and the injection time is based on the injection time of the non-electrically active material ions and the injection density and injection energy (depth) of the non-electrically active material ions in the barrier layer. The injection density of the Ar ions is 3.4E12 cm -2 、3.4E13 cm -2 、3.4E14 cm -2 、1E16cm -2 , and obtain AlGaN barrier layers respectively.

[0062] A gate is prepared in the region where Ar ions are implanted on the upper surface of the AlGaN barrier layer. Finally, the substrate layer is mechanically thinned to less than 300 μm to obtain a normally-off GaN HEMT device.

[0063] The experiment found that with the increase of Ar ion implantation density, the resistance of the normally-off GaN HEMT device first increased and then decreased. It was found that the suitable range of Ar ion implantation density is 1E13~1E15 cm -2 The present invention completely disables the AlGaN barrier and makes it an insulator by controlling the Ar ion implantation density.

[0064] The Vth of the normally-off GaN HEMT device prepared in this embodiment changes from a negative value (<-5V) to a positive value (>1V).

[0065] Example 2

[0066] Preparation Figure 7 The normally-off GaN HEMT device with a first insulating layer of the structure shown in the figure has a specific preparation method comprising the following steps:

[0067] An AlGaN buffer layer and a GaN channel layer are prepared on the upper surface of a substrate layer (thickness is ~1 mm) made of Si, SiC or sapphire.

[0068] An AlGaN initial barrier layer, a source electrode and a drain electrode are prepared on the upper surface of the GaN channel layer.

[0069] The barrier layer is obtained by injecting Ar ions into the AlGaN initial barrier layer, wherein the injection region of the Ar ions in the AlGaN initial barrier layer coincides with the region of the positive projection of the gate on the barrier layer. The injection energy of the Ar ions is 10-100 keV; the injection method includes plasma injection or low-energy ion injection, and the injection time is based on the injection time of the non-electrically active material ions and the injection density and injection energy (depth) of the non-electrically active material ions in the barrier layer. The injection density of the Ar ions is 1E14 cm -2 . An AlGaN barrier layer is obtained.

[0070] The first insulating layer is prepared in the region where Ar ions are implanted on the upper surface of the AlGaN barrier layer; after the first insulating layer is obtained, a gate is prepared on the upper surface of the first insulating layer. Finally, the substrate layer is mechanically thinned to less than 300 μm to obtain a normally-off GaN HEMT device.

[0071] The Vth of the normally-off GaN HEMT device prepared in this embodiment changes from a negative value (<-5V) to a positive value (>1V).

[0072] From the above embodiments, it can be seen that the normally-off high electron mobility transistor provided by the present invention does not etch or damage the barrier layer compared to the above-mentioned "third solution", and has a more stable Vth and an original unetched and undamaged 2DEG layer between the barrier layer and the channel layer. Compared with the above-mentioned "fourth solution", the present invention converts the barrier layer into an insulator by injecting non-electrically active material ions into the barrier layer, thereby rendering the naturally formed 2DEG layer ineffective, and compared to the introduction of electrically active elements (such as chlorine or fluorine atoms), the present invention does not have the defects of decreased mobility due to charge scattering and unstable Vth due to the movement of chlorine or fluorine ions under gate bias. In summary, the normally-off high electron mobility transistor device provided by the present invention has high interface electron mobility, does not have too many Coulomb scattering centers, and has an adjustable and more stable Vth.

[0073] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A normally-off high electron mobility transistor, characterized in that: The invention comprises a substrate layer; a buffer layer arranged on the upper surface of the substrate layer; a channel layer arranged on the upper surface of the buffer layer; a source electrode arranged on part of the upper surface of the channel layer, a drain electrode arranged on part of the upper surface, and a barrier layer arranged on part of the upper surface; a gate electrode arranged on part of the upper surface of the barrier layer; the barrier layer is injected with non-electrically active material ions, the injection area of ​​the non-electrically active material ions in the barrier layer coincides with the positive projection area of ​​the gate electrode on the barrier layer, and the non-electrically active material ions are Ar ions; the thickness of the injection area of ​​the non-electrically active material ions in the barrier layer is equal to the thickness of the barrier layer, and the injection density of the non-electrically active material ions is 1E13-1E15 cm -2 .

2. The normally-off high electron mobility transistor according to claim 1, characterized in that: The injection energy of the non-electrically active material ions is 10-100 keV.

3. The normally-off high electron mobility transistor according to claim 1, characterized in that: Also includes: A first insulating layer is disposed between the barrier layer and the gate, wherein a projection area of ​​the first insulating layer on an upper surface of the barrier layer overlaps with a projection area of ​​the gate on the upper surface of the barrier layer.

4. The normally-off high electron mobility transistor according to claim 3, characterized in that: The material of the first insulating layer includes one or more of SiO2, Al2O3, SiN, AlN or other high dielectric constant dielectric materials, and the dielectric constant of the other high dielectric constant dielectric materials is greater than 9 F / m.

5. The normally-off high electron mobility transistor according to claim 3, characterized in that: The thickness of the first insulating layer is 0-100 nm, and is not 0 nm.

6. The normally-off high electron mobility transistor according to claim 1, characterized in that: The barrier layer includes non-electrically active material ions and a main material, and the main material includes one or more of AlGaN, AlN and InAlN; The material of the channel layer is GaN.

7. The method for preparing a normally-off high electron mobility transistor according to any one of claims 1 to 6, characterized in that: The following steps are involved: Sequentially preparing a buffer layer and a channel layer on the upper surface of the substrate layer; Preparing a source electrode, a drain electrode and an initial barrier layer on the upper surface of the channel layer; Injecting non-electrically active material ions into the initial barrier layer to obtain a barrier layer; the injection region of the non-electrically active material ions into the initial barrier layer coincides with the positive projection region of the gate on the barrier layer; A gate is prepared on the upper surface of the region of the barrier layer where the non-electrically active material ions are implanted.

8. The preparation method according to claim 7, characterized in that: The implantation method includes plasma implantation or low-energy ion implantation.

9. The preparation method according to claim 7, characterized in that: After obtaining the barrier layer and before preparing the gate, the method further includes: preparing a first insulating layer on the upper surface of the region where the barrier layer is injected with non-electrically active material ions; after obtaining the first insulating layer, preparing the gate on the upper surface of the first insulating layer.

Citation Information

Patent Citations

  • Insulated gate AlGaN / GaN high electron mobility transistor with multi-channel fin structure

    CN105355657A

  • Normally-closed InAlN / GaN HMET device with p-GaN gate structure and preparation method thereof

    CN110518068A

  • Enhanced gallium nitride high-electron-mobility transistor and preparation method thereof

    CN111668101A