A method for manufacturing a TBC structure back contact battery and a back contact battery

Through in-situ boron-doped single crystal silicon layer annealing technology and PECVD plus annealing, the problem of poor passivation effect of the back contact battery of the TBC structure is solved, the process flow is simplified, the cost is reduced, and the battery conversion efficiency is improved.

CN118380513BActive Publication Date: 2024-11-08HUAIAN JIETAI NEW ENERGY TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410810021.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-11-08
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

When the existing TBC structure back contact battery uses boron-doped polycrystalline silicon in the P region, the passivation effect is poor, which affects the battery conversion efficiency, and has many high-temperature steps and high cost.

Method used

The single crystal silicon layer annealing technology with in-situ boron doped is used to form a high-concentration boron doped P region, and the high-temperature process is reduced by PECVD annealing. All metal electrodes combined with BC structure are designed on the back side to avoid blocking sunlight and simplify the process. process.

Benefits of technology

The boron doping concentration on the surface of P zone is improved, the silicon wafer damage is reduced, the battery preparation process is simplified, the production cost is reduced, and the battery conversion efficiency is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118380513B_ABST
    Figure CN118380513B_ABST
Patent Text Reader

Abstract

The present application discloses a manufacturing method of a TBC structure back contact cell and a back contact cell, which belongs to the technical field of solar cell manufacturing. The back contact cell of the present application adopts a boron-doped single crystal silicon method in the P region, avoiding the problem of poor passivation effect caused by the common boron-doped polycrystalline silicon as the P region; at the same time, the boron doping is performed by annealing the polycrystalline silicon layer non-in-situ boron doping, so that the boron concentration on the surface of the P region is the highest, which can effectively utilize the advantages of the BC structure cell, so that the metal slurry can be sintered at a shallow depth to obtain a better ohmic contact, reducing the damage and recombination of the P region.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of solar cell manufacturing, and more specifically, to a manufacturing method of a TBC structure back-contact cell and a back-contact cell. Background Art

[0002] The principle of solar cells that directly convert light energy into electrical energy lies in the artificially manufactured PN junction structure, which can selectively separate the photogenerated carriers, thereby generating a potential difference between the two regions. In the design and production of solar cells, increasing the open circuit voltage, short circuit current, and fill factor FF are common means to improve the photoelectric conversion efficiency.

[0003] The PN junction and metal contact electrode of the back contact (BC) solar cell are designed on the back of the cell. There is no electrode shielding on the front surface, which can increase the short-circuit current of the cell. At the same time, all metal grid lines are designed on the back, without considering the influence of shading. During the component packaging process, the cells can be arranged more closely together, improving the packaging density of the component, thereby increasing the conversion efficiency of the component.

[0004] At present, the preparation of BC structure batteries generally involves the preparation and removal of masks, as well as two high-temperature processes of boron diffusion and phosphorus diffusion. The process is complex and the cost is high. At the same time, the use of boron-doped polysilicon in the P region makes it difficult to improve the passivation effect, thus affecting the overall conversion efficiency of the battery.

[0005] In the prior art, Patent No. CN114823991A discloses a method for preparing a back-contact battery and a back-contact battery. The application uses the PECVD method to prepare the P region of boron-doped amorphous silicon and the N region of phosphorus-doped amorphous silicon, respectively, and finally completes the doping by annealing. However, the P region of the structure produced is still in the form of boron-doped polysilicon, and it is difficult to improve the passivation effect.

[0006] Patent No. CN112864275A discloses a method for preparing an IBC battery, an IBC battery and a solar cell module. The application forms a P region by diffusing boron on monocrystalline silicon, and forms an N region by LPCVD plus phosphorus diffusion, but it has many high-temperature steps, which is not conducive to cost control; the boron concentration on the surface of the P region is low, which is not conducive to the formation of better ohmic contact between the silicon wafer and the metal slurry during the sintering process; the high-power laser will form a large-area contact with the surface of the silicon wafer, which is easy to cause damage to it. Summary of the invention

[0007] 1. Technical problem to be solved by the invention

[0008] In view of the above-mentioned deficiencies in the prior art, the present application provides a method for manufacturing a TBC structure back-contact cell and a back-contact cell. The TBC structure solar cell adopts a boron-doped single-crystal silicon in the P region, thereby avoiding the poor passivation effect caused by the common boron-doped polycrystalline silicon as the P region. At the same time, non-in-situ boron-doped polycrystalline silicon layer annealing is used for boron doping, so that the boron concentration on the surface of the P region is the highest, which can effectively utilize the advantages of the BC structure cell, so that the metal slurry can be sintered at a shallow depth to obtain better ohmic contact, thereby reducing damage and recombination in the P region.

[0009] 2. Technical solution

[0010] The content of this application is used to introduce concepts in a brief form, which will be described in detail in the detailed implementation section below. The content of this application is not intended to identify the key features or essential features of the technical solution claimed for protection, nor is it intended to limit the scope of the technical solution claimed for protection.

[0011] In order to achieve the above objectives, the technical solution provided by this application is:

[0012] As a first aspect of the present application, the present application provides a method for manufacturing a TBC structure back contact battery, comprising the following steps:

[0013] S01, double-sided polishing of the silicon wafer and cleaning;

[0014] S02, growing an in-situ boron-doped amorphous silicon layer on both sides of the silicon wafer, and then growing a first barrier layer on the in-situ boron-doped amorphous silicon layer;

[0015] S03, etching the first barrier layer on the back side of the silicon wafer to form an interdigitated pattern, setting the etched area as the second area, and setting the remaining barrier layer area as the first area;

[0016] S04, etching the silicon wafer to form a groove in the second region;

[0017] S05, sequentially growing a tunneling oxide layer, an intrinsic amorphous silicon layer, an in-situ phosphorus-doped amorphous silicon layer, and a second barrier layer in the groove and on the first barrier layer in the first region;

[0018] S06, performing annealing treatment on the silicon wafer, so that the first region of the boron-doped single crystal silicon forms a P region, the second region of the phosphorus-doped single crystal silicon forms an N region, and the amorphous silicon layer is transformed into a polycrystalline silicon layer;

[0019] S07, removing the second barrier layer on the first region, and burning a channel between the first region and the second region;

[0020] S08, making the front side of the silicon wafer into a single crystal velvet surface, and removing the phosphorus-doped polysilicon layer, the tunneling oxide layer, the first barrier layer and the boron-doped polysilicon layer in the first region in sequence; finally, cleaning the silicon wafer and removing the second barrier layer on the second region;

[0021] S09, growing a passivation layer on the front and back surfaces of the silicon wafer;

[0022] S10. Make an electrode on the back side of the silicon wafer to obtain a TBC structure back contact cell.

[0023] Furthermore, the in-situ phosphorus-doped amorphous silicon layer is an amorphous silicon layer doped with high concentration in-situ phosphorus at a concentration of more than 4E20.

[0024] Furthermore, the thickness of the in-situ boron-doped amorphous silicon layer is 50-100 nm, and the thickness of the first barrier layer is 45-55 nm.

[0025] Furthermore, the first barrier layer and the second barrier layer are made of materials that are not easily reactive with alkali.

[0026] Furthermore, the first barrier layer and the second barrier layer are silicon dioxide or silicon nitride.

[0027] Furthermore, in step S04, the silicon wafer is placed in an alkaline solution for alkaline etching, wherein the alkaline solution is a NaOH solution or a KOH solution.

[0028] Furthermore, in step S04, the in-situ boron-doped amorphous silicon layer and a portion of the single crystal silicon layer in the second region are removed to form a groove.

[0029] Furthermore, step S05 uses silane and nitrous oxide as reaction gases to grow a tunneling oxide layer in the groove and on the first barrier layer in the first area, then grows an intrinsic amorphous silicon layer on the tunneling oxide layer, then grows an in-situ phosphorus-doped amorphous silicon layer on the intrinsic amorphous silicon layer, and finally grows a second barrier layer on the in-situ phosphorus-doped amorphous silicon layer.

[0030] Furthermore, the thickness of the tunneling oxide layer is 1-2 nm, the thickness of the intrinsic amorphous silicon layer is 150-300 nm, the thickness of the in-situ phosphorus-doped amorphous silicon layer is 30-60 nm, and the thickness of the second barrier layer is 48-52 nm.

[0031] Furthermore, in step S06, the silicon wafer is annealed at a temperature of 900-1000° C. for 30-60 minutes.

[0032] Furthermore, in step S03, the first barrier layer is etched using a laser, and in step S07, a green laser with a wavelength of 532 nm is used to remove the second barrier layer on the first region.

[0033] Furthermore, step S08 performs a wet process, using the sequence of alkali solution-acid solution-alkali solution-acid solution to sequentially remove the phosphorus-doped polysilicon layer, the tunneling oxide layer, the first barrier layer and the boron-doped polysilicon layer in the first region, and finally remove the second barrier layer on the second region.

[0034] Furthermore, step S08 uses NaOH texturing solution to make a single crystal texture surface on the front side of the silicon wafer, and at the same time etches out the phosphorus-doped polysilicon layer in the first area, and then uses HF solution to remove the tunneling oxide layer and the first barrier layer on the first area, and then uses alkaline solution to remove the boron-doped polysilicon layer on the first area, and finally uses HF solution to clean the entire wafer, and at the same time removes the second barrier layer on the second area.

[0035] As a second aspect of the present application, the present application provides a TBC structure back contact battery, which is manufactured using the method provided in the present application.

[0036] Furthermore, the main structure of the battery is N-type doped single crystal silicon; the front side is a single crystal velvet structure, the N region on the back side is a phosphorus-heavy doped polysilicon layer plus a tunneling oxide layer structure, and the P region is a boron-doped single crystal silicon structure; the surfaces of the front and back sides are covered with a passivation film composed of aluminum oxide, silicon nitride, and silicon oxynitride.

[0037] 3. Beneficial effects

[0038] Compared with the existing known technologies, the technical solution provided by this application has the following significant effects:

[0039] (1) The present application prepares a boron-doped amorphous silicon layer on the back surface of the BC battery as the doping source of the P region, so that the surface boron doping concentration of the P region is the highest; at the same time, the amorphous silicon layer also serves as a buffer layer between the laser and the N region, avoiding direct contact between the high-power laser and the N region, thereby reducing damage to the silicon wafer.

[0040] (2) The present application uses PECVD plus annealing to prepare the P region and the N region, which reduces the high-temperature process and the use and loss of quartz parts, while reducing the plating on the front side, thereby simplifying the battery preparation process and saving production costs.

[0041] (3) This application combines the characteristics of BC structure batteries in which all metal electrodes are on the back and will not block sunlight, uses boron-doped amorphous silicon as the doping source, and finally removes the amorphous silicon part, so that the surface of the P zone is the area with the highest doping concentration. This can increase the slurry coverage area, reduce the sintering depth, reduce damage to the silicon substrate, and reduce recombination. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] The drawings constituting a part of this application are used to provide a further understanding of this application, so that other features, purposes and advantages of this application become more obvious. The illustrative embodiment drawings and their descriptions of this application are used to explain this application and do not constitute an improper limitation on this application.

[0043] In addition, throughout the drawings, the same or similar reference numerals represent the same or similar elements. It should be understood that the drawings are schematic and that the components and elements are not necessarily drawn to scale.

[0044] In the attached picture:

[0045] Figure 1-Figure 10 This is a schematic diagram of the structural changes of the TBC structure back contact battery of this application;

[0046] Fig.11 This is a flow chart for preparing the TBC structure back contact battery of this application.

[0047] Explanation of the symbols in the schematic diagram:

[0048] 1. Silicon wafer; 21. In-situ boron-doped amorphous silicon layer; 22. Boron-doped polysilicon layer; 3. First barrier layer; 4. First region; 5. Second region; 6. Tunneling oxide layer; 7. Intrinsic amorphous silicon layer; 81. In-situ phosphorus-doped amorphous silicon layer; 82. Phosphorus-doped polysilicon layer; 9. Second barrier layer; 10. N region; 11. P region; 12. Channel; 13. Passivation layer; 14. Electrode. DETAILED DESCRIPTION

[0049] Embodiments of the present application will be described in more detail below with reference to the accompanying drawings. Although certain embodiments of the present application are shown in the accompanying drawings, it should be understood that the present application can be implemented in various forms, and should not be construed as being limited to the embodiments set forth herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present application. It should be understood that the drawings and embodiments of the present application are only for exemplary purposes and are not intended to limit the scope of protection of the present application.

[0050] It should also be noted that, for ease of description, only the parts related to the invention are shown in the drawings. In the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other.

[0051] The present application will be described in detail below with reference to the accompanying drawings and in combination with embodiments.

[0052] The present invention discloses a method for manufacturing a TBC structure back contact battery, which specifically comprises the following steps: using a polished N-type single crystal silicon wafer as a silicon substrate, growing an in-situ boron-doped amorphous silicon layer on the back of the polished silicon wafer by PECVD, and then growing a barrier layer thereon. After removing the barrier layer in a part of the area by laser, alkaline etching is performed to etch a groove in the area burnt by the laser, and then growing a tunnel oxide layer and an intrinsic amorphous silicon layer by PECVD, and then growing a layer of 4E20 (i.e., 4×10 20 cm -3 ) and finally grow a barrier layer on the in-situ phosphorus-doped amorphous silicon layer. After annealing, doping is performed. Annealing will rearrange the silicon atoms in the amorphous silicon. During the annealing and cooling process, the silicon atoms in each small range of the amorphous silicon layer will be arranged in order to form a lattice, so that the amorphous silicon layer is transformed into a polycrystalline silicon layer. At the same time, the high temperature annealing process will cause the boron in the amorphous silicon to enter the single crystal silicon substrate under the region, resulting in a higher concentration of boron in this area. The outermost layer of the boron element is 3 electrons, which is one less than the 4 electrons of the silicon element. Therefore, in the area with higher boron doping, the main carrier is positively charged holes. Therefore, the doping of the boron element replacing the silicon element in the lattice is called P-type doping, and the corresponding area with a higher boron content will form a P region. Similarly, the phosphorus in the amorphous silicon diffuses evenly into the amorphous silicon layer. After the temperature is lowered, all the amorphous silicon layers become polycrystalline silicon layers to form an N region. Then use laser to etch away the outermost barrier layer of the P region, and burn a channel in the P region and N region at the same time. Then carry out the wet process step, using the sequence of alkali-acid-alkali-acid, remove the N-type polysilicon layer in the back P region, the P-type polysilicon layer and the barrier layer between the two polysilicon layers, and the barrier layer in the N region in turn, and turn the front side into a single crystal velvet surface. Finally, double-sided ALD, front and back film, printing and sintering processes are carried out to make solar cells.

[0053] The TBC structure back contact cell structure finally manufactured by the present application is: the main structure is N-type doped single crystal silicon; the front side is a single crystal velvet structure, the back side N area is a phosphorus heavily doped polysilicon layer plus a tunneling oxide layer structure, and the P area is a boron doped single crystal silicon structure. At the same time, the front and back surfaces are covered with a passivation film composed of aluminum oxide, silicon nitride, and silicon oxynitride.

[0054] The TBC structure back contact cell manufactured by this application has a simple process and few high-temperature steps, which is conducive to reducing manufacturing costs. The P region is a boron-doped single crystal silicon structure, which avoids the poor passivation effect of the boron Poly structure. At the same time, the in-situ doped amorphous silicon layer is used as the doping layer, so that the surface of the P region is the highest concentration area, which is conducive to the metallization contact in the printing process; the N region retains the structure of the tunneling oxide layer of the current TOPCon battery covered with a high concentration of phosphorus Poly, so that electrons can pass selectively and reduce recombination, which is conducive to improving the battery conversion efficiency.

[0055] Example 1

[0056] See also Fig.11 A method for manufacturing a TBC structure back contact battery of this embodiment comprises the following steps:

[0057] S01, prepare a piece of original silicon wafer 1 with a resistivity of 12Ω·cm and a thickness of 200μm, polish it on both sides, and clean it. Figure 1 shown.

[0058] S02, the silicon wafer 1 is placed in a PECVD device, a 100nm in-situ boron-doped amorphous silicon layer 21 is grown on both sides of the polished silicon wafer 1, and then a 45nm first barrier layer 3 is grown thereon; the first barrier layer 3 is silicon dioxide, such as Figure 2 shown.

[0059] S03, using laser to etch the first barrier layer 3 on the back side, forming a P region-N region-P region-N region interdigital pattern on the first barrier layer 3 on the back side, and setting the laser etched area as the second area 5, and the remaining barrier layer area as the first area 4, such as Figure 3 shown.

[0060] S04, placing the silicon wafer 1 in an alkaline solution, performing alkaline etching at a temperature of 80° C. for 20 minutes, etching a groove with a depth of 2 μm in the second region 5, and removing the in-situ boron-doped amorphous silicon layer 21 and part of the single crystal silicon layer in the second region 5, such as Figure 4 As shown, the alkaline solution is a NaOH solution.

[0061] S05, using the PECVD equipment again, using silane and laughing gas as reaction gases, growing a tunnel oxide layer 6 with a thickness of 2nm on the first barrier layer 3 in the groove and the first region 4, then growing a layer of intrinsic amorphous silicon layer 7 with a thickness of 300nm on the tunnel oxide layer 6, and then growing a layer of in-situ phosphorus-doped amorphous silicon layer 81 with a thickness of 60nm on the intrinsic amorphous silicon layer 7. Finally, growing a second barrier layer 9 with a thickness of 50nm on the in-situ phosphorus-doped amorphous silicon layer 81, wherein the second barrier layer 9 is silicon dioxide, such as Figure 5 shown.

[0062] S06. The silicon wafer 1 is annealed at 1000°C for 60 minutes for doping. The high temperature process in the first half of the annealing process will push the boron atoms in the amorphous silicon into the single crystal silicon at the bottom of the region, resulting in a higher boron concentration in this region. The positively charged holes become majority carriers with a higher content, and the negatively charged electrons become minority carriers with a lower content, so that the first region of the boron-doped single crystal silicon forms a P region 11, and the second region doped with phosphorus forms an N region 10. Different from the P region 11, there is a tunneling oxide layer 6 between the phosphorus-doped amorphous silicon layer and the single crystal silicon substrate, which can effectively prevent the phosphorus atoms from diffusing into the single crystal silicon layer behind, so that most of the phosphorus atoms remain in the amorphous silicon layer. The cooling process in the second half of the annealing process will cause the silicon atoms in the amorphous silicon to rearrange in order to form a lattice, so that the amorphous silicon layer is transformed into a polycrystalline silicon layer (that is, the in-situ boron-doped amorphous silicon layer 21 is transformed into a boron-doped polycrystalline silicon layer 22, and the in-situ phosphorus-doped amorphous silicon layer 81 is transformed into a phosphorus-doped polycrystalline silicon layer 82). Figure 6 shown.

[0063] S07, using a green laser with a wavelength of 532nm, remove the second barrier layer 9 on the first region 4. At the same time, burn a channel 12 between the first region 4 and the second region 5, such as Figure 7 shown.

[0064] S08, using NaOH texturing solution to make a single crystal texture surface on the front side of the silicon wafer 1, and etching away the phosphorus-doped polysilicon layer 82 remaining in the first region 4, and then using HF solution to remove the thinner tunneling oxide layer 6 and the first barrier layer 3 on the first region 4, and then using alkaline solution to remove the thinner boron-doped polysilicon layer 22 covering the first region 4, and finally using HF to clean the entire wafer, and at the same time completely remove the second barrier layer 9 remaining in the second region 5, as shown in FIG. Figure 8 shown.

[0065] S09, placing the silicon wafer in the ALD device, growing a 6nm thick Al2O3 film on the front and back sides of the silicon wafer. Then placing it in the PECVD device, generating a 90nm thick anti-reflection film of a composite structure of silicon nitride and silicon oxynitride on the front and back sides. The composite anti-reflection film and the Al2O3 film form a passivation layer 13, such as Fig. 9 shown.

[0066] S10, on the back of the silicon wafer, use a screen printer to print silver paste in the P region and the N region, and then sinter it at a temperature of 900°C to form a silver electrode 14 to obtain a solar cell. Fig.10 shown.

[0067] Example 2

[0068] A method for manufacturing a TBC structure back contact battery of this embodiment includes the following steps:

[0069] S01. Prepare a raw silicon wafer 1 with a resistivity of 2Ω·cm and a thickness of 150μm, polish both sides, and clean it.

[0070] S02, placing the silicon wafer 1 into a PECVD device, growing a 50nm in-situ boron-doped amorphous silicon layer 21 on both sides of the polished silicon wafer 1, and then growing a 55nm first barrier layer 3 thereon; the first barrier layer 3 is silicon nitride.

[0071] S03. Use laser to etch the back part of the first barrier layer 3 to form a P region-N region-P region-N region interdigitated pattern on the back first barrier layer 3, and set the laser etched area as the second area 5, and the remaining barrier layer area as the first area 4.

[0072] S04, placing the silicon wafer 1 in an alkaline solution, performing alkaline etching at a temperature of 80° C. for 10 minutes, etching a groove with a depth of 1 μm in the second region 5, and removing the in-situ boron-doped amorphous silicon layer 21 and part of the single crystal silicon layer in the second region 5, wherein the alkaline solution is a KOH solution.

[0073] S05. Using the PECVD equipment again, using silane and nitrous oxide as reaction gases, a tunnel oxide layer 6 with a thickness of 1 nm is grown on the first barrier layer 3 in the groove and the first region 4, and then a layer of intrinsic amorphous silicon layer 7 with a thickness of 150 nm is grown on the tunnel oxide layer 6, and then a layer of in-situ phosphorus-doped amorphous silicon layer 81 with a thickness of 30 nm is grown on the intrinsic amorphous silicon layer 7. Finally, a second barrier layer 9 with a thickness of 50 nm is grown on the in-situ phosphorus-doped amorphous silicon layer 81, and the second barrier layer 9 is silicon nitride.

[0074] S06, annealing the silicon wafer 1 at 900°C for 30 minutes for doping. The high temperature process in the first half of the annealing process will push the boron atoms in the amorphous silicon into the single crystal silicon at the bottom of the region, resulting in a higher concentration of boron in this region, and the positively charged holes become the majority carriers with a higher content, and the negatively charged electrons become the minority carriers with a lower content, so that the first region of the boron-doped single crystal silicon forms a P region 11, and the second region of phosphorus-doped forms an N region 10. Different from the P region 11, there is a tunneling oxide layer 6 between the phosphorus-doped amorphous silicon layer and the single crystal silicon substrate, which can effectively prevent the phosphorus atoms from diffusing into the single crystal silicon layer behind, so that most of the phosphorus atoms remain in the amorphous silicon layer. The cooling process in the second half of the annealing process will cause the silicon atoms in the amorphous silicon to rearrange in order to form a lattice, so that the amorphous silicon layer is transformed into a polycrystalline silicon layer.

[0075] S07 , using a green laser with a wavelength of 532 nm to remove the second barrier layer 9 on the first region 4 , and at the same time burn a channel 12 between the first region 4 and the second region 5 .

[0076] S08. Use NaOH texturing solution to make a single crystal texture surface on the front side of the silicon wafer 1, and at the same time etch away the phosphorus-doped polysilicon layer 82 remaining in the first area 4, and then use HF solution to remove the thinner tunneling oxide layer 6 and the first barrier layer 3 on the first area 4, and then use alkaline solution to remove the thinner boron-doped polysilicon layer 22 covering the first area 4, and finally use HF to clean the entire wafer, and at the same time completely remove the second barrier layer 9 remaining in the second area 5.

[0077] S09, placing the silicon wafer in an ALD device, growing a 4nm thick Al2O3 film on the front and back sides of the silicon wafer. Then placing it in a PECVD device, growing a 60nm thick anti-reflection film of a composite structure of silicon nitride and silicon oxynitride on the front and back sides, the composite anti-reflection film and the Al2O3 film forming a passivation layer 13.

[0078] S10. On the back of the silicon wafer, use a screen printer to print silver paste in the P region and the N region, and then perform sintering at a temperature of 800° C. to form a silver electrode 14 to obtain a solar cell.

[0079] Example 3

[0080] A method for manufacturing a TBC structure back contact battery of this embodiment includes the following steps:

[0081] S01. Prepare a raw silicon wafer 1 with a resistivity of 6Ω·cm and a thickness of 180μm, polish both sides, and clean it.

[0082] S02, placing the silicon wafer 1 into a PECVD device, growing an 80nm in-situ boron-doped amorphous silicon layer 21 on both sides of the polished silicon wafer 1, and then growing a 50nm first barrier layer 3 thereon; the first barrier layer 3 is silicon dioxide.

[0083] S03. Use laser to etch the back part of the first barrier layer 3 to form a P region-N region-P region-N region interdigitated pattern on the back first barrier layer 3, and set the laser etched area as the second area 5, and the remaining barrier layer area as the first area 4.

[0084] S04, placing the silicon wafer 1 in an alkaline solution, performing alkaline etching at a temperature of 80° C. for 15 minutes, etching a groove with a depth of 1.5 μm in the second region 5, and removing the in-situ boron-doped amorphous silicon layer 21 and part of the single crystal silicon layer in the second region 5, wherein the alkaline solution is a NaOH solution.

[0085] S05. Using the PECVD equipment again, using silane and laughing gas as reaction gases, a tunnel oxide layer 6 with a thickness of 1.5 nm is grown on the first barrier layer 3 in the groove and the first region 4, and then a layer of intrinsic amorphous silicon layer 7 with a thickness of 200 nm is grown on the tunnel oxide layer 6, and then a layer of in-situ phosphorus-doped amorphous silicon layer 81 with a thickness of 50 nm is grown on the intrinsic amorphous silicon layer 7. Finally, a second barrier layer 9 with a thickness of 50 nm is grown on the in-situ phosphorus-doped amorphous silicon layer 81, and the second barrier layer 9 is silicon nitride.

[0086] S06, annealing the silicon wafer 1 at 950°C for 40 minutes for doping. The high temperature process in the first half of the annealing process will push the boron atoms in the amorphous silicon into the single crystal silicon at the bottom of the region, resulting in a higher concentration of boron in this region, and the positively charged holes become the majority carriers with a higher content, and the negatively charged electrons become the minority carriers with a lower content, so that the first region of the boron-doped single crystal silicon forms a P region 11, and the second region of phosphorus-doped forms an N region 10. Different from the P region 11, there is a tunneling oxide layer 6 between the phosphorus-doped amorphous silicon layer and the single crystal silicon substrate, which can effectively prevent the phosphorus atoms from diffusing into the single crystal silicon layer behind, so that most of the phosphorus atoms remain in the amorphous silicon layer. The cooling process in the second half of the annealing process will cause the silicon atoms in the amorphous silicon to rearrange in order to form a lattice, so that the amorphous silicon layer is transformed into a polycrystalline silicon layer.

[0087] S07 , using a green laser with a wavelength of 532 nm to remove the second barrier layer 9 on the first region 4 , and at the same time burn a channel 12 between the first region 4 and the second region 5 .

[0088] S08. Use NaOH texturing solution to make a single crystal texture surface on the front side of the silicon wafer 1, and at the same time etch away the phosphorus-doped polysilicon layer 82 remaining in the first area 4, and then use HF solution to remove the thinner tunneling oxide layer 6 and the first barrier layer 3 on the first area 4, and then use alkaline solution to remove the thinner boron-doped polysilicon layer 22 covering the first area 4, and finally use HF to clean the entire wafer, and at the same time completely remove the second barrier layer 9 remaining in the second area 5.

[0089] S09, placing the silicon wafer in an ALD device, growing a 5nm thick Al2O3 film on the front and back sides of the silicon wafer. Then placing it in a PECVD device, generating an 80nm thick anti-reflection film of a composite structure of silicon nitride and silicon oxynitride on the front and back sides, the composite anti-reflection film and the Al2O3 film forming a passivation layer 13.

[0090] S10. On the back of the silicon wafer, use a screen printer to print silver paste in the P region and the N region, and then perform sintering at a temperature of 850° C. to form a silver electrode 14 to obtain a solar cell.

[0091] The above description is only some preferred embodiments of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the embodiments of the present application is not limited to the technical solutions formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the above invention concept. For example, the above features are replaced with (but not limited to) technical features with similar functions disclosed in the embodiments of the present application to form a technical solution.

Claims

1. A method for manufacturing a TBC structure back contact battery, characterized in that: The following steps are involved: S01, double-sided polishing of the silicon wafer (1) and cleaning thereof; S02, growing an in-situ boron-doped amorphous silicon layer (21) on both sides of the silicon wafer (1), and then growing a first barrier layer (3) on the in-situ boron-doped amorphous silicon layer (21); S03, etching the first barrier layer (3) on the back side of the silicon wafer (1) to form a cross-finger pattern, setting the etched area as the second area (5), and setting the remaining barrier layer area as the first area (4); S04, etching the silicon wafer (1) so as to form a groove in the second region (5); S05, sequentially growing a tunneling oxide layer (6), an intrinsic amorphous silicon layer (7), an in-situ phosphorus-doped amorphous silicon layer (81), and a second barrier layer (9) in the groove and on the first barrier layer (3) in the first region (4); S06, annealing the silicon wafer (1) at a temperature of 900-1000° C. for 30-60 minutes, so that the first region of the boron-doped single-crystalline silicon forms a P region (11), the in-situ boron-doped amorphous silicon layer (21) is transformed into a boron-doped polycrystalline silicon layer (22), and the phosphorus in the in-situ phosphorus-doped amorphous silicon layer (81) is uniformly diffused into the amorphous silicon layer. After the temperature is lowered, the intrinsic amorphous silicon layer (7) and the in-situ phosphorus-doped amorphous silicon layer (81) are transformed into a polycrystalline silicon layer, thereby forming an N region (10); S07, removing the second barrier layer (9) on the first region (4), and burning a channel (12) between the first region (4) and the second region (5); S08, forming a single crystal velvet surface on the front side of the silicon wafer (1), and at the same time sequentially removing the phosphorus-doped polysilicon layer (82), the tunneling oxide layer (6), the first barrier layer (3), and the boron-doped polysilicon layer (22) in the first region (4); finally, cleaning the silicon wafer (1) and removing the second barrier layer (9) on the second region (5); S09, growing a passivation layer (13) on the front and back surfaces of the silicon wafer (1); S10, forming an electrode (14) on the back side of the silicon wafer to obtain a TBC structure back contact cell.

2. The method for manufacturing a TBC structure back contact battery according to claim 1, characterized in that: The in-situ phosphorus-doped amorphous silicon layer (81) is an amorphous silicon layer doped with high concentration in-situ phosphorus at a concentration of more than 4E20.

3. The method for manufacturing a TBC structure back contact battery according to claim 1, characterized in that: The thickness of the in-situ boron-doped amorphous silicon layer (21) is 50-100 nm, and the thickness of the first barrier layer (3) is 45-55 nm.

4. The method for manufacturing a TBC structure back contact battery according to claim 2, characterized in that: The first barrier layer (3) and the second barrier layer (9) are made of materials that are not easily reactive with alkali.

5. The method for manufacturing a TBC structure back contact battery according to claim 4, characterized in that: The first barrier layer (3) and the second barrier layer (9) are silicon dioxide or silicon nitride.

6. The method for manufacturing a TBC structure back contact battery according to claim 4, characterized in that: Step S04: placing the silicon wafer (1) in an alkaline solution for alkaline etching, wherein the alkaline solution is a NaOH solution or a KOH solution.

7. The method for manufacturing a TBC structure back contact battery according to claim 6, characterized in that: In step S04, the in-situ boron-doped amorphous silicon layer (21) and a portion of the single crystal silicon layer in the second region (5) are removed to form a groove.

8. The method for manufacturing a TBC structure back contact battery according to claim 7, characterized in that: In step S05, silane and nitrous oxide are used as reaction gases to grow a tunneling oxide layer (6) on the first barrier layer (3) in the groove and the first region (4), then grow an intrinsic amorphous silicon layer (7) on the tunneling oxide layer (6), then grow an in-situ phosphorus-doped amorphous silicon layer (81) on the intrinsic amorphous silicon layer (7), and finally grow a second barrier layer (9) on the in-situ phosphorus-doped amorphous silicon layer (81).

9. The method for manufacturing a TBC structure back contact battery according to claim 8, characterized in that: The thickness of the tunneling oxide layer (6) is 1-2 nm, the thickness of the intrinsic amorphous silicon layer (7) is 150-300 nm, the thickness of the in-situ phosphorus-doped amorphous silicon layer (81) is 30-60 nm, and the thickness of the second barrier layer (9) is 48-52 nm.

10. The method for manufacturing a TBC structure back contact battery according to claim 9, characterized in that: In step S03, the first barrier layer (3) is etched using a laser, and in step S07, a green laser with a wavelength of 532 nm is used to remove the second barrier layer (9) on the first region (4).

11. The method for manufacturing a TBC structure back contact battery according to claim 10, characterized in that: Step S08 is a wet process step, in which the phosphorus-doped polysilicon layer (82), the tunnel oxide layer (6), the first barrier layer (3) and the boron-doped polysilicon layer (22) of the first region (4) are removed in sequence using an alkali solution-an acid solution-an alkali solution-an acid solution, and finally the second barrier layer (9) on the second region (5) is removed.

12. The method for manufacturing a TBC structure back contact battery according to claim 10, characterized in that: In step S08, a NaOH texturing solution is used to make a single crystal textured surface on the front side of the silicon wafer (1), and the phosphorus-doped polysilicon layer (82) in the first region (4) is etched away at the same time. Then, an HF solution is used to remove the tunneling oxide layer (6) and the first barrier layer (3) on the first region (4), and then an alkaline solution is used to remove the boron-doped polysilicon layer (22) on the first region (4). Finally, an HF solution is used to clean the entire wafer, and the second barrier layer (9) on the second region (5) is removed at the same time.

13. A TBC structure back contact battery, characterized in that: The product is prepared by the method according to any one of claims 1 to 12.

14. A TBC structure back contact battery according to claim 13, characterized in that: The main structure of the battery is N-type doped single crystal silicon; the front side is a single crystal velvet structure, the N region on the back side is a phosphorus-heavy doped polysilicon layer plus a tunneling oxide layer structure, and the P region is a boron-doped single crystal silicon structure; the surfaces of the front and back sides are covered with a passivation film composed of aluminum oxide, silicon nitride, and silicon oxynitride.

Citation Information

Patent Citations

  • Preparation method of IBC cell, IBC cell and solar cell module

    CN112864275A

  • Preparation method of back contact battery and back contact battery

    CN114823991A

  • Method for manufacturing back contact solar cell

    CN103794679A

  • Patterned passivation contact solar cell and manufacturing method thereof

    CN112164728A

  • Local passivation contact IBC battery structure and preparation method thereof

    CN113611755A