Flexible high temperature resistant glass and preparation method thereof
By using non-metallic oxides, metal oxides, carbonates and clarifiers in the preparation of flexible high-temperature resistant glass, and using vertical overflow pressing and horizontal rotation stretching forming processes, the glass defect problem is solved and improved Its flexibility and high temperature resistance are suitable for a variety of high-end applications.
Patent Information
- Application Number
- CN202410854340.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-06-28
AI Technical Summary
Existing flexible high-temperature resistant glasses are prone to microscopic or macroscopic defects during the preparation process, affecting their flexibility and high-temperature resistance.
Using non-metal oxides, metal oxides, carbonates and clarifiers as raw materials, the temperature and thickness of each stage are controlled to reduce the glass by using a process of vertical overflow pressing, 90° horizontal rotation and secondary stretching forming. The defects of the improvement of flexibility and high temperature resistance.
It significantly improves the flexibility and high-temperature resistance of flexible high-temperature glass, with a critical bending curvature radius below 6μm and a high-temperature resistance of above 750℃. It is suitable for foldable screens, solar panels and spacecraft fields.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of glass materials, and in particular to a flexible high temperature resistant glass and a preparation method thereof. Background Art
[0002] As electronic information display has higher and higher requirements for glass substrates, flexible high-temperature resistant glass has emerged. Flexible high-temperature resistant glass is a new type of glass material with good bendability and high temperature resistance. In addition, it has the advantages of good flatness, high hardness, scratch resistance, good touch, and stable chemical properties. It is mainly used in folding screen mobile phones, solar panels, and aerospace.
[0003] The preparation methods of flexible high temperature resistant glass include float process, overflow down-draw method, slit down-draw method and re-draw method. Among them, overflow down-draw method is a commonly used process for preparing flexible high temperature resistant glass. However, since flexible high temperature resistant glass is extremely thin, it is easy to produce microscopic or macroscopic defects, which greatly affects its flexibility and high temperature resistance. Summary of the invention
[0004] The present invention provides a flexible high temperature resistant glass and a preparation method thereof, which solves the problem of poor flexibility and high temperature resistance of the flexible high temperature resistant glass in the related art.
[0005] The technical solution of the present invention is as follows:
[0006] A flexible high temperature resistant glass, the raw materials comprising the following components in parts by weight: 85-95 parts of non-metallic oxide, 4-17.3 parts of metal oxide, 0.8-3.27 parts of carbonate, and 0.6-1.3 parts of clarifier;
[0007] The clarifier includes sodium pyroantimonate and / or sodium chloride.
[0008] As a further technical solution, the non-metallic oxide is quartz sand.
[0009] As a further technical solution, the clarifier includes 0.1-0.7 parts of sodium pyroantimonate and 0.3-0.9 parts of sodium chloride.
[0010] The present invention limits the clarifier to 0.1-0.7 parts of sodium pyroantimonate and 0.3-0.9 parts of sodium chloride, which further improves the flexibility and high temperature resistance of the glass.
[0011] As a further technical solution, the thickness is 8~20μm; the critical curvature radius of bending is 2~6μm; and the high temperature resistance is 750~900℃.
[0012] As a further technical solution, the metal oxide includes the following components in parts by mass: 2 to 8.5 parts of zirconium dioxide, 1 to 1.8 parts of yttrium trioxide, and 1 to 7 parts of cerium oxide;
[0013] The carbonate includes the following components in parts by mass: 0.34-1.71 parts of sodium carbonate, 0.25-1.23 parts of lithium carbonate, 0.15-0.88 parts of potassium carbonate, and 0.06-0.25 parts of cesium carbonate.
[0014] As a further technical solution, it is composed of the following components in mass percentage: 85%~95% silicon dioxide, 2%~8.5% zirconium dioxide, 1%~1.8% yttrium oxide, 1%~7% cerium oxide, 0.2%~1% sodium oxide, 0.1%~0.5% lithium oxide, 0.1%~0.6% potassium oxide, and 0.05%~0.22% cesium oxide.
[0015] The present invention also proposes a method for preparing a flexible high-temperature resistant glass, comprising the following steps: melting raw materials to obtain glass liquid, and processing the glass liquid into a shape to obtain the flexible high-temperature resistant glass.
[0016] As a further technical solution, the melting temperature is 1780~1900°C.
[0017] As a further technical solution, the processing and forming is specifically as follows: the glass liquid is subjected to a vertical overflow pressing forming, and then horizontally rotated, subjected to a secondary stretching forming, and annealed to obtain a flexible high temperature resistant glass.
[0018] As a further technical solution, the temperature of the one-time vertical overflow pressing is 1470~1600℃;
[0019] The angle of horizontal rotation is 90°, and the temperature during horizontal rotation is 1460-1550°C;
[0020] The temperature of the secondary stretching is 1380-1510°C;
[0021] The annealing temperature is 980-1210°C.
[0022] As a further technical solution, a vertical overflow pressing is performed once to form the steel sheet to a thickness of 0.3 to 1 mm.
[0023] The forming method adopts one vertical overflow pressing + 90° horizontal rotation + secondary horizontal thinning, and by controlling the temperature and forming thickness at each stage, the micro and macro defects of the glass are reduced, and the flexibility and high temperature resistance of the glass are further improved.
[0024] The working principle and beneficial effects of the present invention are:
[0025] The present invention uses non-metallic oxides, metal oxides, carbonates and clarifiers as glass raw materials, wherein the clarifier uses sodium pyroantimonate and / or sodium chloride, to provide a glass with good flexibility and high temperature resistance, which can be widely used in foldable and high temperature resistant fields. In addition, it also has certain radiation resistance, can be applied to various spacecraft in space, and can be directly exposed in space, and can also be applied to the industrial field, expanding the scope of use of transparent glass materials, and has important application prospects. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] The parameters of the raw materials in the following examples and comparative examples are as follows:
[0028] The particle size of the quartz sand is 0.1 mm and the content of silicon dioxide is ≥ 99.5 wt%.
[0029] Example 1
[0030] S1, after uniformly mixing 85 parts of quartz sand, 8.5 parts of zirconium dioxide, 1.8 parts of yttrium trioxide, 1.71 parts of sodium carbonate, 0.88 parts of potassium carbonate, 0.25 parts of cesium carbonate and 1 part of sodium chloride, add the mixture into a heating furnace and melt at 1820°C to obtain glass liquid;
[0031] S2. The glass liquid is subjected to a vertical overflow pressing at 1530°C to obtain a glass with a thickness of 0.5 mm. Then, a 1500°C rotating roller is used to change the glass from a vertical direction to a horizontal direction. A secondary stretching is performed at 1450°C to obtain a glass with a thickness of 13 μm. Finally, it is annealed at 1050°C and cooled to room temperature to obtain a flexible high-temperature resistant glass.
[0032] Example 2
[0033] S1, after uniformly mixing 85 parts of quartz sand, 8.5 parts of zirconium dioxide, 1.8 parts of yttrium trioxide, 2.55 parts of cerium oxide, 1.71 parts of sodium carbonate, 1.23 parts of lithium carbonate, 0.88 parts of potassium carbonate, 0.06 parts of cesium carbonate, 0.2 parts of sodium pyroantimonate and 0.8 parts of sodium chloride, adding the mixture into a heating furnace and melting at 1820°C to obtain glass liquid;
[0034] S2. The glass liquid is subjected to a vertical overflow pressing at 1530°C to obtain a glass with a thickness of 0.5 mm. Then, a 1500°C rotating roller is used to change the glass from a vertical direction to a horizontal direction. A secondary stretching is performed at 1450°C to obtain a glass with a thickness of 13 μm. Finally, it is annealed at 1050°C and cooled to room temperature to obtain a flexible high-temperature resistant glass.
[0035] Example 3
[0036] S1, 95 parts of quartz sand, 2 parts of zirconium dioxide, 1.8 parts of yttrium trioxide, 1 part of cerium oxide, 0.34 parts of sodium carbonate, 0.1 parts of lithium carbonate, 0.15 parts of potassium carbonate, 0.25 parts of cesium carbonate, 0.5 parts of sodium pyroantimonate, and 0.4 parts of sodium chloride were mixed evenly, and then added into a heating furnace and melted at 1820°C to obtain glass liquid;
[0037] S2. The glass liquid is subjected to a vertical overflow pressing at 1530°C to obtain a glass with a thickness of 0.5 mm. Then, a 1500°C rotating roller is used to change the glass from a vertical direction to a horizontal direction. A secondary stretching is performed at 1450°C to obtain a glass with a thickness of 13 μm. Finally, it is annealed at 1050°C and cooled to room temperature to obtain a flexible high-temperature resistant glass.
[0038] Example 4
[0039] S1, 88.6 parts of quartz sand, 2 parts of zirconium dioxide, 1 part of yttrium trioxide, 7 parts of cerium oxide, 1.36 parts of sodium carbonate, 0.25 parts of lithium carbonate, 0.44 parts of potassium carbonate, 0.23 parts of cesium carbonate, 0.5 parts of sodium pyroantimonate, and 0.4 parts of sodium chloride were mixed evenly, added into a heating furnace and melted at 1780°C to obtain glass liquid;
[0040] S2. The glass liquid is subjected to a vertical overflow pressing at 1470°C to obtain a glass with a thickness of 1 mm. A rotating roller at 1460°C is then used to change the glass from a vertical direction to a horizontal direction. A secondary stretching is performed at 1380°C to obtain a glass with a thickness of 20 μm. Finally, it is annealed at 980°C and cooled to room temperature to obtain a flexible high-temperature resistant glass.
[0041] Example 5
[0042] S1, 88 parts of quartz sand, 5.2 parts of zirconium dioxide, 1.5 parts of yttrium trioxide, 4 parts of cerium oxide, 1.03 parts of sodium carbonate, 0.74 parts of lithium carbonate, 0.44 parts of potassium carbonate, 0.11 parts of cesium carbonate, 0.4 parts of sodium pyroantimonate, and 0.6 parts of sodium chloride were mixed evenly, and then added into a heating furnace and melted at 1900° C. to obtain glass liquid;
[0043] S2. The glass liquid is subjected to a vertical overflow pressing at 1600°C to obtain a glass with a thickness of 0.3 mm. A rotating roller at 1550°C is then used to change the glass from a vertical direction to a horizontal direction. A secondary stretching is performed at 1510°C to obtain a glass with a thickness of 8 μm. Finally, the glass is annealed at 1210°C and cooled to room temperature to obtain a flexible high-temperature resistant glass.
[0044] Example 6
[0045] S1, after uniformly mixing 85 parts of quartz sand, 8.5 parts of zirconium dioxide, 1.8 parts of yttrium trioxide, 2.55 parts of cerium oxide, 1.71 parts of sodium carbonate, 1.23 parts of lithium carbonate, 0.88 parts of potassium carbonate, 0.06 parts of cesium carbonate, 0.2 parts of sodium pyroantimonate and 0.8 parts of sodium chloride, adding the mixture into a heating furnace and melting at 1820°C to obtain glass liquid;
[0046] S2. The glass liquid is subjected to a vertical overflow pressing at 1650°C to obtain a glass with a thickness of 0.5 mm. Then, a 1500°C rotating roller is used to change the glass from a vertical direction to a horizontal direction. A secondary stretching is performed at 1450°C to obtain a glass with a thickness of 13 μm. Finally, it is annealed at 1050°C and cooled to room temperature to obtain a flexible high-temperature resistant glass.
[0047] Example 7
[0048] S1, after uniformly mixing 85 parts of quartz sand, 8.5 parts of zirconium dioxide, 1.8 parts of yttrium trioxide, 2.55 parts of cerium oxide, 1.71 parts of sodium carbonate, 1.23 parts of lithium carbonate, 0.88 parts of potassium carbonate, 0.06 parts of cesium carbonate, 0.2 parts of sodium pyroantimonate and 0.8 parts of sodium chloride, adding the mixture into a heating furnace and melting at 1820°C to obtain glass liquid;
[0049] S2. The glass liquid is subjected to a vertical overflow pressing at 1410°C to obtain a glass with a thickness of 0.5 mm. Then, a 1500°C rotating roller is used to change the glass from a vertical direction to a horizontal direction. A secondary stretching is performed at 1450°C to obtain a glass with a thickness of 13 μm. Finally, it is annealed at 1050°C and cooled to room temperature to obtain a flexible high-temperature resistant glass.
[0050] Example 8
[0051] S1, 88 parts of quartz sand, 5.2 parts of zirconium dioxide, 1.5 parts of yttrium trioxide, 4 parts of cerium oxide, 1.03 parts of sodium carbonate, 0.74 parts of lithium carbonate, 0.44 parts of potassium carbonate, 0.11 parts of cesium carbonate, 0.4 parts of sodium pyroantimonate, and 0.6 parts of sodium chloride were mixed evenly, and then added into a heating furnace and melted at 1900° C. to obtain glass liquid;
[0052] S2. The glass liquid is subjected to a vertical overflow pressing at 1600°C to obtain a glass with a thickness of 0.3 mm. A rotating roller at 1550°C is then used to change the glass from a vertical direction to a horizontal direction. A secondary stretching is performed at 1530°C to obtain a glass with a thickness of 8 μm. Finally, the glass is annealed at 1210°C and cooled to room temperature to obtain a flexible high-temperature resistant glass.
[0053] Example 9
[0054] S1, 88 parts of quartz sand, 5.2 parts of zirconium dioxide, 1.5 parts of yttrium trioxide, 4 parts of cerium oxide, 1.03 parts of sodium carbonate, 0.74 parts of lithium carbonate, 0.44 parts of potassium carbonate, 0.11 parts of cesium carbonate, 0.4 parts of sodium pyroantimonate, and 0.6 parts of sodium chloride were mixed evenly, and then added into a heating furnace and melted at 1900° C. to obtain glass liquid;
[0055] S2. The glass liquid is subjected to a vertical overflow pressing at 1600°C to obtain a glass with a thickness of 0.3 mm. A 1550°C rotating roller is used to change the glass from a vertical direction to a horizontal direction. A secondary stretching is performed at 1330°C to obtain a glass with a thickness of 8 μm. Finally, it is annealed at 1210°C and cooled to room temperature to obtain a flexible high-temperature resistant glass.
[0056] Example 10
[0057] S1, 85 parts of quartz sand, 8.5 parts of zirconium dioxide, 1.8 parts of yttrium trioxide, 2.55 parts of cerium oxide, 1.71 parts of sodium carbonate, 1.23 parts of lithium carbonate, 0.88 parts of potassium carbonate, 0.06 parts of cesium carbonate and 1 part of sodium pyroantimonate were mixed evenly, added into a heating furnace and melted at 1820°C to obtain glass liquid;
[0058] S2. The glass liquid is subjected to a vertical overflow pressing at 1530°C to obtain a glass with a thickness of 0.5 mm. Then, a 1500°C rotating roller is used to change the glass from a vertical direction to a horizontal direction. A secondary stretching is performed at 1450°C to obtain a glass with a thickness of 13 μm. Finally, it is annealed at 1050°C and cooled to room temperature to obtain a flexible high-temperature resistant glass.
[0059] Embodiment 11
[0060] S1, after uniformly mixing 85 parts of quartz sand, 8.5 parts of zirconium dioxide, 1.8 parts of yttrium trioxide, 2.55 parts of cerium oxide, 1.71 parts of sodium carbonate, 1.23 parts of lithium carbonate, 0.88 parts of potassium carbonate, 0.06 parts of cesium carbonate and 1 part of sodium chloride, add the mixture into a heating furnace and melt at 1820°C to obtain glass liquid;
[0061] S2. The glass liquid is subjected to a vertical overflow pressing at 1530°C to obtain a glass with a thickness of 0.5 mm. Then, a 1500°C rotating roller is used to change the glass from a vertical direction to a horizontal direction. A secondary stretching is performed at 1450°C to obtain a glass with a thickness of 13 μm. Finally, it is annealed at 1050°C and cooled to room temperature to obtain a flexible high-temperature resistant glass.
[0062] Example 12
[0063] S1, 85 parts of quartz sand, 8.5 parts of zirconium dioxide, 1.8 parts of yttrium trioxide, 2.55 parts of cerium oxide, 1.71 parts of sodium carbonate, 1.23 parts of lithium carbonate, 0.88 parts of potassium carbonate, 0.06 parts of cesium carbonate, 0.1 parts of sodium pyroantimonate, and 0.9 parts of sodium chloride were mixed evenly, and then added into a heating furnace and melted at 1820°C to obtain glass liquid;
[0064] S2. The glass liquid is subjected to a vertical overflow pressing at 1530°C to obtain a glass with a thickness of 0.5 mm. Then, a 1500°C rotating roller is used to change the glass from a vertical direction to a horizontal direction. A secondary stretching is performed at 1450°C to obtain a glass with a thickness of 13 μm. Finally, it is annealed at 1050°C and cooled to room temperature to obtain a flexible high-temperature resistant glass.
[0065] Example 13
[0066] S1, after uniformly mixing 85 parts of quartz sand, 8.5 parts of zirconium dioxide, 1.8 parts of yttrium trioxide, 2.55 parts of cerium oxide, 1.71 parts of sodium carbonate, 1.23 parts of lithium carbonate, 0.88 parts of potassium carbonate, 0.06 parts of cesium carbonate, 0.7 parts of sodium pyroantimonate and 0.3 parts of sodium chloride, add the mixture into a heating furnace and melt at 1820°C to obtain glass liquid;
[0067] S2. The glass liquid is subjected to a vertical overflow pressing at 1530°C to obtain a glass with a thickness of 0.5 mm. Then, a 1500°C rotating roller is used to change the glass from a vertical direction to a horizontal direction. A secondary stretching is performed at 1450°C to obtain a glass with a thickness of 13 μm. Finally, it is annealed at 1050°C and cooled to room temperature to obtain a flexible high-temperature resistant glass.
[0068] Embodiment 14
[0069] S1, after uniformly mixing 85 parts of quartz sand, 8.5 parts of zirconium dioxide, 1.8 parts of yttrium trioxide, 2.55 parts of cerium oxide, 1.71 parts of sodium carbonate, 1.23 parts of lithium carbonate, 0.88 parts of potassium carbonate, 0.06 parts of cesium carbonate, 0.2 parts of sodium pyroantimonate and 0.8 parts of sodium chloride, adding the mixture into a heating furnace and melting at 1820°C to obtain glass liquid;
[0070] S2. The glass liquid is subjected to a vertical overflow pressing at 1530°C to obtain a glass with a thickness of 1.5 mm. Then, a 1500°C rotating roller is used to change the glass from a vertical direction to a horizontal direction. A secondary stretching is performed at 1450°C to obtain a glass with a thickness of 13 μm. Finally, it is annealed at 1050°C and cooled to room temperature to obtain a flexible high-temperature resistant glass.
[0071] Embodiment 15
[0072] S1, after uniformly mixing 85 parts of quartz sand, 8.5 parts of zirconium dioxide, 1.8 parts of yttrium trioxide, 2.55 parts of cerium oxide, 1.71 parts of sodium carbonate, 1.23 parts of lithium carbonate, 0.88 parts of potassium carbonate, 0.06 parts of cesium carbonate, 0.2 parts of sodium pyroantimonate and 0.8 parts of sodium chloride, adding the mixture into a heating furnace and melting at 1820°C to obtain glass liquid;
[0073] S2. The glass liquid is subjected to a vertical overflow pressing at 1530°C to obtain a glass with a thickness of 0.1 mm. Then, a 1500°C rotating roller is used to change the glass from a vertical direction to a horizontal direction. A secondary stretching is performed at 1450°C to obtain a glass with a thickness of 13 μm. Finally, it is annealed at 1050°C and cooled to room temperature to obtain a flexible high-temperature resistant glass.
[0074] The softening point of the flexible high temperature resistant glass obtained in Examples 1 to 15 was tested according to the method in GB / T 28195-2011, and recorded as the high temperature resistant temperature; the critical curvature radius of bending was tested according to the method in T / CSTM 00409-2021, and the test results are recorded in Table 1.
[0075] Table 1 Critical curvature radius and high temperature resistant temperature of flexible high temperature resistant glass
[0076]
[0077] It can be seen from Table 1 that the critical curvature radius of the flexible high temperature resistant glass provided by the present invention is below 6 μm, the high temperature resistant temperature is above 750° C., and the glass has good flexibility and high temperature resistance.
[0078] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A flexible high temperature resistant glass, characterized in that: The raw materials include the following components in parts by weight: 85-95 parts of non-metallic oxide, 4-17.3 parts of metal oxide, 0.8-3.27 parts of carbonate, and 0.6-1.3 parts of clarifier; The non-metallic oxide is quartz sand; The clarifier includes 0.1-0.7 parts of sodium pyroantimonate and 0.3-0.9 parts of sodium chloride; The metal oxide comprises the following components in parts by mass: 2 to 8.5 parts of zirconium dioxide, 1 to 1.8 parts of yttrium trioxide, and 1 to 7 parts of cerium oxide; The carbonate comprises the following components in parts by mass: 0.34-1.71 parts of sodium carbonate, 0.25-1.23 parts of lithium carbonate, 0.15-0.88 parts of potassium carbonate, and 0.06-0.25 parts of cesium carbonate; The preparation method comprises the following steps: melting raw materials to obtain glass liquid, and processing the glass liquid into a shape to obtain flexible high temperature resistant glass; The processing and forming is specifically as follows: the glass liquid is subjected to a vertical overflow pressing and forming, and then horizontally rotated, subjected to a secondary stretching and forming, and annealed to obtain a flexible high temperature resistant glass; The temperature of the primary vertical overflow pressing is 1470-1600°C; The temperature of the secondary stretching is 1380-1510°C; The mold is formed by a single vertical overflow press to a thickness of 0.3~1mm.
2. The flexible high temperature resistant glass according to claim 1, characterized in that: The thickness is 8~20μm; the critical curvature radius of bending is 2~6μm; the high temperature resistance is 750~900℃.
3. The flexible high temperature resistant glass according to claim 1, characterized in that: It is composed of the following components in percentage by mass: 85%~95% silicon dioxide, 2%~8.5% zirconium dioxide, 1%~1.8% yttrium oxide, 1%~7% cerium oxide, 0.2%~1% sodium oxide, 0.1%~0.5% lithium oxide, 0.1%~0.6% potassium oxide, and 0.05%~0.22% cesium oxide.
4. The method for preparing a flexible high temperature resistant glass according to any one of claims 1 to 3, characterized in that: The following steps are involved: After the raw materials are melted, glass liquid is obtained, and the glass liquid is processed and shaped to obtain flexible high-temperature resistant glass.
5. The method for preparing a flexible high temperature resistant glass according to claim 4, characterized in that: The melting temperature is 1780~1900℃.
6. The method for preparing a flexible high temperature resistant glass according to claim 4, characterized in that: The processing and forming is specifically as follows: the glass liquid is subjected to a vertical overflow pressing forming, and then horizontally rotated, subjected to a secondary stretching forming, and annealed to obtain a flexible high temperature resistant glass.
7. The method for preparing a flexible high temperature resistant glass according to claim 6, characterized in that: The temperature of the primary vertical overflow pressing is 1470-1600°C; The angle of horizontal rotation is 90°, and the temperature during horizontal rotation is 1460-1550°C; The temperature of the secondary stretching is 1380-1510°C; The annealing temperature is 980-1210°C.
8. The method for preparing a flexible high temperature resistant glass according to claim 6, characterized in that: The mold is formed by a single vertical overflow press to a thickness of 0.3~1mm.