A barium sulfate polymer composite material and preparation method thereof

By modifying nanobarium sulfate and adding multi-walled carbon nanotubes and glass fibers, the brittleness and dispersion of epoxy resins and barium sulfate in the field of high-performance materials are solved, and the mechanical properties and toughness of the materials are significantly improved.

CN118388926BActive Publication Date: 2024-11-19CHONGQING LUYU MINING DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410502888.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-25
Publication Date
2024-11-19
Estimated Expiration
2044-04-25

AI Technical Summary

Technical Problem

The curing system of epoxy resin has high brittleness, poor toughness and insufficient impact resistance. The poor dispersion of barium sulfate limits its application in the field of high-performance materials.

Method used

The surface of nanobarium sulfate was coated with methyl methacrylate, modified with ethylenediamine, and grafted polyethyleneimine, combined with 4,4-diaminodiphenylmethane curing agent, to prepare a high curing density with a high curing density Epoxy resin composite material and multi-walled carbon nanotubes and glass fibers are added to improve mechanical properties.

Benefits of technology

It significantly improves the mechanical properties of epoxy resin, enhances the compatibility between nanobarium sulfate and epoxy resin, improves the toughness and curing density of the material, and improves the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a barium sulfate polymer composite material and a preparation method thereof in the technical field of material preparation. The barium sulfate polymer composite material comprises the following components in parts by weight: 80-100 parts of epoxy resin, 10-20 parts of modified nano barium sulfate, 6-8 parts of multi-walled carbon nanotubes, 7-9 parts of glass fiber, 20-30 parts of acetone, and 10-15 parts of 4,4-diaminodiphenylmethane curing agent. The invention proposes coating the surface of nano barium sulfate with methyl methacrylate, then modifying it with ethylenediamine, and finally grafting polyethyleneimine to the surface to obtain modified nano barium sulfate, and coordinating with 4,4-diaminodiphenylmethane curing agent to prepare an epoxy resin composite material with high curing density, and adding multi-walled carbon nanotubes and glass fiber at the same time to further improve the mechanical properties of the epoxy resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material preparation, and specifically refers to a barium sulfate polymer composite material and a preparation method thereof. Background Art

[0002] Epoxy resin is one of the most widely used thermosetting materials. Compared with other thermosetting resins, epoxy resin has special properties, such as low shrinkage during curing, short curing time, excellent adhesion, high mechanical strength and chemical corrosion resistance. It is widely used in aerospace, marine engineering, chemical anti-corrosion, environmentally friendly coatings, people's livelihood and civilian fields. However, the curing system of epoxy resin has the disadvantages of high brittleness, poor toughness and impact resistance, which limits its application in key material fields with high requirements for mechanical properties. Barium sulfate is widely used in coatings, papermaking, rubber, plastics and textile industries due to its advantages of easy development, low cost, non-toxicity and strong stability. Nano barium sulfate has higher application value. It not only has the advantages of ordinary barium sulfate, but also has great application prospects in polymer materials, nonlinear optics, medical and catalysis. The application value and specific application fields of nano barium sulfate are closely related to its own dispersibility. At present, the nano barium sulfate prepared by traditional methods has the disadvantages of poor dispersibility and serious particle agglomeration, which greatly limits its application.

[0003] The existing technology currently has the following main problems: the performance of epoxy resin is poor and the dispersibility of barium sulfate is poor. Summary of the invention

[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a barium sulfate polymer composite material and a preparation method thereof. The present invention proposes to coat the surface of nano-barium sulfate with methyl methacrylate, then modify it with ethylenediamine, and finally graft polyethyleneimine to the surface to obtain modified nano-barium sulfate, and cooperate with 4,4-diaminodiphenylmethane curing agent to prepare an epoxy resin composite material with higher curing density, and at the same time add multi-walled carbon nanotubes and glass fibers to further improve the mechanical properties of the epoxy resin.

[0005] In order to achieve the above-mentioned purpose, the technical scheme adopted by the present invention is as follows: The present invention proposes a barium sulfate polymer composite material and a preparation method thereof, wherein the barium sulfate polymer composite material comprises the following components in parts by weight: 80-100 parts of epoxy resin, 10-20 parts of modified nano barium sulfate, 6-8 parts of multi-walled carbon nanotubes, 7-9 parts of glass fiber, 20-30 parts of acetone, and 10-15 parts of 4,4-diaminodiphenylmethane curing agent.

[0006] Furthermore, the preparation method of the modified nano-barium sulfate comprises the following steps:

[0007] (1) Add barium chloride and sodium sulfate to 100 mL of deionized water, stir to fully dissolve, then transfer to a flask, add oleic acid, heat to 80-90°C, stir at 600 rpm for 30-40 min, filter after completion, wash with deionized water 3 times, and vacuum dry at 50°C to obtain oleic acid-modified nano-barium sulfate;

[0008] (2) Add the oleic acid-modified nano-barium sulfate obtained in step (1) into a flask, add methyl methacrylate, add divinylbenzene, and perform ultrasonic treatment for 10-20 min at a power of 400 W. Then, add initiator azobisisobutyronitrile, react at 60° C. and 400 rpm for 40-60 min. Take the precipitate, wash it with deionized water three times, then add it to 100 mL of methanol, add ethylenediamine, and react at 60° C. for 20-24 h to obtain ethylenediamine-modified nano-barium sulfate.

[0009] (3) Add polyethyleneimine to methanol to obtain a polyethyleneimine solution, add the ethylenediamine-modified nano-barium sulfate obtained in step (1) to the polyethyleneimine solution, stir magnetically at room temperature for 20-24 hours at a stirring speed of 300-400 rpm, add 1 wt % glutaraldehyde aqueous solution, continue stirring for 30-40 minutes, and wash with deionized water three times to obtain modified nano-barium sulfate.

[0010] Furthermore, in step (1), the mass ratio of the barium chloride to the sodium sulfate is 1:2-3.

[0011] Furthermore, in step (1), the volume ratio of oleic acid to deionized water is 1-2:100.

[0012] Furthermore, in step (2), the volume ratio of divinylbenzene to methyl methacrylate is 1:15-20.

[0013] Furthermore, in step (2), the mass ratio of the oleic acid-modified nano-barium sulfate to azobisisobutyronitrile is 1:1-2.

[0014] Furthermore, in step (2), the mass ratio of the oleic acid-modified nano-barium sulfate to ethylenediamine is 1:2-4.

[0015] Furthermore, in step (3), the mass fraction of the polyethyleneimine in methanol is 2%-3%.

[0016] Furthermore, in step (3), the mass concentration of the ethylenediamine-modified nano-barium sulfate in the polyethyleneimine solution is 20-30 g / L.

[0017] Furthermore, in step (3), the volume ratio of the glutaraldehyde aqueous solution to the polyethyleneimine solution is 3-4:1.

[0018] The present invention provides a method for preparing a barium sulfate polymer composite material, which specifically comprises the following steps:

[0019] Take multi-walled carbon nanotubes and glass fibers and add them to acetone, stir for 2-3 hours, then add epoxy resin, continue stirring for 3-4 hours, add modified nano barium sulfate and 4,4-diaminodiphenylmethane curing agent, stir for 1-2 hours, and cure at room temperature for 10-20 hours to obtain a barium sulfate polymer composite material.

[0020] The beneficial effects achieved by the present invention are as follows:

[0021] The invention uses oleic acid as a medium to coat the surface of nano barium sulfate with methyl methacrylate, then uses ethylenediamine to modify the surface, and finally grafts polyethyleneimine onto the surface to obtain modified nano barium sulfate, and cooperates with 4,4-diaminodiphenylmethane curing agent to prepare an epoxy resin composite material with high curing density, and simultaneously adds multi-walled carbon nanotubes and glass fibers to further improve the mechanical properties of the epoxy resin; by modifying the nano barium sulfate, the surface chemical structure of the nano barium sulfate is changed to form functional groups such as ester groups, amide groups and amino groups, and these functional groups can react with epoxy groups to form covalent bonds. bond, enhance the interfacial interaction between nano-barium sulfate and epoxy resin, improve the compatibility of nano-barium sulfate and epoxy resin, and at the same time, the rich amino groups on the modified nano-barium sulfate can effectively cure epoxy resin, and cooperate with 4,4-diaminodiphenylmethane curing agent to prepare epoxy resin composite materials with high curing density; glass fiber reinforced epoxy resin has the advantages of light weight and high strength, but poor toughness. The introduction of multi-walled carbon nanotubes has the characteristics of small volume, high aspect ratio and excellent mechanical properties, which can be effectively integrated with the resin matrix, significantly affecting the generation and expansion of microcracks inside the matrix, and making up for the toughness of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The tensile strength test results of Examples 1-3 and Comparative Examples 1-2 of the present invention are shown in FIG.

[0023] Figure 2 The compressive strength test results of Examples 1-3 and Comparative Examples 1-2 of the present invention are shown in FIG.

[0024] Figure 3 The bending strength test results of Examples 1-3 and Comparative Examples 1-2 of the present invention are shown in FIG.

[0025] Figure 4 This is a scanning electron microscope image of the barium sulfate polymer composite material prepared in Example 1 of the present invention.

[0026] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0028] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.

[0029] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.

[0030] Example 1

[0031] A barium sulfate polymer composite material comprises the following components in parts by weight: 80 parts of epoxy resin, 10 parts of modified nano barium sulfate, 6 parts of multi-walled carbon nanotubes, 7 parts of glass fiber, 20 parts of acetone, and 10 parts of 4,4-diaminodiphenylmethane curing agent.

[0032] The preparation method of modified nano barium sulfate comprises the following steps:

[0033] (1) Take 1g of barium chloride and 2g of sodium sulfate and add them to 100mL of deionized water, stir to fully dissolve, then transfer to a flask, add 1mL of oleic acid, heat to 80°C, stir at 600rpm for 30min, filter after completion, wash with deionized water 3 times, and vacuum dry at 50°C to obtain oleic acid-modified nano-barium sulfate;

[0034] (2) Take 500 mg of the oleic acid-modified nano-barium sulfate obtained in step (1) and add it to a flask, add 3 mL of methyl methacrylate, add 200 µL of divinylbenzene, and ultrasonicate for 10 min at a power of 400 W, then add 500 mg of azobisisobutyronitrile, react at 60 ° C and 400 rpm for 40 min, take the precipitate and wash it with deionized water three times, then add it to 100 mL of methanol, add 1 g of ethylenediamine, and react at 60 ° C for 20 h to obtain ethylenediamine-modified nano-barium sulfate;

[0035] (3) Add polyethyleneimine to methanol to prepare a polyethyleneimine solution with a mass fraction of 2%, add 1 g of the ethylenediamine-modified nano-barium sulfate obtained in step (2) to 50 mL of the polyethyleneimine solution, stir magnetically at room temperature for 20 h at a stirring speed of 300 rpm, add 150 mL of a 1 wt % glutaraldehyde aqueous solution, continue stirring for 30 min, and wash with deionized water three times to obtain modified nano-barium sulfate.

[0036] This embodiment provides a method for preparing a barium sulfate polymer composite material, which specifically includes the following steps:

[0037] Multi-walled carbon nanotubes and glass fibers were added to acetone and stirred for 2 h. Then epoxy resin was added and stirred for 3 h. Modified nano barium sulfate and 4,4-diaminodiphenylmethane curing agent were added and stirred for 1 h. The mixture was cured at room temperature for 10 h to obtain a barium sulfate polymer composite material.

[0038] Example 2

[0039] A barium sulfate polymer composite material comprises the following components in parts by weight: 100 parts of epoxy resin, 20 parts of modified nano barium sulfate, 8 parts of multi-walled carbon nanotubes, 9 parts of glass fiber, 30 parts of acetone, and 15 parts of 4,4-diaminodiphenylmethane curing agent.

[0040] The preparation method of modified nano barium sulfate comprises the following steps:

[0041] (1) Take 1g of barium chloride and 3g of sodium sulfate and add them to 100mL of deionized water, stir to fully dissolve, then transfer to a flask, add 2mL of oleic acid, heat to 90°C, stir at 600rpm for 40min, filter after completion, wash with deionized water 3 times, and vacuum dry at 50°C to obtain oleic acid-modified nano-barium sulfate;

[0042] (2) Take 500 mg of the oleic acid-modified nano-barium sulfate obtained in step (1) and add it to a flask, add 4 mL of methyl methacrylate, add 200 µL of divinylbenzene, and ultrasonicate for 20 min at a power of 400 W, then add 1000 mg of azobisisobutyronitrile, react at 60 ° C and 400 rpm for 60 min, take the precipitate and wash it with deionized water three times, then add it to 100 mL of methanol, add 2 g of ethylenediamine, and react at 60 ° C for 24 h to obtain ethylenediamine-modified nano-barium sulfate;

[0043] (3) Add polyethyleneimine to methanol to prepare a polyethyleneimine solution with a mass fraction of 3%, add 2 g of the ethylenediamine-modified nano-barium sulfate obtained in step (2) to 50 mL of the polyethyleneimine solution, stir magnetically at room temperature for 24 h at a stirring speed of 400 rpm, add 200 mL of a 1 wt % glutaraldehyde aqueous solution, continue stirring for 40 min, and wash with deionized water three times to obtain modified nano-barium sulfate.

[0044] This embodiment provides a method for preparing a barium sulfate polymer composite material, which specifically includes the following steps:

[0045] Multi-walled carbon nanotubes and glass fibers were added to acetone and stirred for 3 h. Then epoxy resin was added and stirred for 4 h. Modified nano barium sulfate and 4,4-diaminodiphenylmethane curing agent were added and stirred for 2 h. The mixture was cured at room temperature for 20 h to obtain a barium sulfate polymer composite material.

[0046] Example 3

[0047] A barium sulfate polymer composite material comprises the following components in parts by weight: 90 parts of epoxy resin, 15 parts of modified nano barium sulfate, 7 parts of multi-walled carbon nanotubes, 8 parts of glass fiber, 25 parts of acetone, and 13 parts of 4,4-diaminodiphenylmethane curing agent.

[0048] The preparation method of modified nano barium sulfate comprises the following steps:

[0049] (1) Take 1g of barium chloride and 2.5g of sodium sulfate and add them to 100mL of deionized water, stir to fully dissolve, then transfer to a flask, add 1.5mL of oleic acid, heat to 85°C, stir at 600rpm for 35min, filter after completion, wash with deionized water 3 times, and vacuum dry at 50°C to obtain oleic acid-modified nano-barium sulfate;

[0050] (2) Take 500 mg of the oleic acid-modified nano-barium sulfate obtained in step (1) and add it to a flask, add 3.5 mL of methyl methacrylate, add 200 µL of divinylbenzene, and ultrasonicate for 15 min at a power of 400 W, then add 750 mg of azobisisobutyronitrile, react at 60 ° C and 400 rpm for 50 min, take the precipitate and wash it with deionized water three times, then add it to 100 mL of methanol, add 1.5 g of ethylenediamine, and react at 60 ° C for 22 h to obtain ethylenediamine-modified nano-barium sulfate;

[0051] (3) Add polyethyleneimine to methanol to prepare a polyethyleneimine solution with a mass fraction of 2.5%, add 1.5 g of the ethylenediamine-modified nano-barium sulfate obtained in step (2) to 50 mL of the polyethyleneimine solution, stir magnetically at room temperature for 22 h at a stirring speed of 350 rpm, add 180 mL of a 1 wt % glutaraldehyde aqueous solution, continue stirring for 35 min, and wash with deionized water three times to obtain modified nano-barium sulfate.

[0052] This embodiment provides a method for preparing a barium sulfate polymer composite material, which specifically includes the following steps:

[0053] Multi-walled carbon nanotubes and glass fibers were added to acetone and stirred for 2.5 hours. Then epoxy resin was added and stirring was continued for 3.5 hours. Modified nano barium sulfate and 4,4-diaminodiphenylmethane curing agent were added and stirred for 1.5 hours. The mixture was cured at room temperature for 15 hours to obtain a barium sulfate polymer composite material.

[0054] Comparative Example 1

[0055] This comparative example provides a barium sulfate polymer composite material and a preparation method thereof, which differs from Example 1 in that the nano-barium sulfate is not modified, that is, the modified nano-barium sulfate is replaced by nano-barium sulfate, and the remaining components and component contents are the same as those in Example 1.

[0056] Comparative Example 2

[0057] This comparative example provides a barium sulfate polymer composite material and a preparation method thereof. The difference between the comparative example and Example 1 is that multi-walled carbon nanotubes and glass fibers are not added, and the remaining components and component contents are the same as those in Example 1.

[0058] Experimental Example 1

[0059] The tensile strength test of Examples 1-3 of the present invention and Comparative Examples 1 and 2 was carried out with reference to the performance test method of resin casting body in GB / T2567-2008, and a universal material testing machine was used to apply a static tensile load along the axial direction of the sample at a uniform speed until the sample breaks or reaches a predetermined elongation. During the whole process, the load applied to the sample and the elongation of the sample were measured to determine the tensile stress. The test speed was 10 mm / min, and the tensile strength was calculated according to the following formula:

[0060] σ t =P / (b×h)

[0061] Where: t is the tensile strength (Mpa), P is the breaking load (N), b is the specimen width (mm), and h is the specimen thickness (mm).

[0062] Experimental Example 2

[0063] The compressive strength test of Examples 1-3 of the present invention and Comparative Examples 1 and 2 was carried out with reference to the performance test method of resin casting body in GB / T2567-2008, and a universal material testing machine was used to compress the sample along the axial direction at a constant rate until the sample was destroyed or the height was reduced to a predetermined value. During the whole process, the load applied to the sample and the height or strain of the sample were measured to determine the compressive stress. The test speed was 5 mm / min, and the tensile strength was calculated according to the following formula:

[0064] σ c =P / (b×h)

[0065] Where: t is the compressive strength (MPa), P is the breaking load (N), b is the specimen width (mm), and h is the specimen thickness (mm).

[0066] Experimental Example 3

[0067] The bending strength test of Examples 1-3 of the present invention and Comparative Examples 1 and 2 was carried out with reference to the performance test method of resin casting body in GB / T2567-2008, using a universal material testing machine, using unconstrained support, three-point bending, and a constant loading rate to make the sample destroyed or reach a predetermined deflection value. During the whole process, the load applied to the sample and the deflection of the sample were measured to determine the bending strength. The bending strength was calculated according to the following formula:

[0068] σ e =3P×L / (2b×h 2 )

[0069] Where: e is the bending strength (Mpa), P is the breaking load (N), L is the span (mm), b is the specimen width (mm), and h is the specimen thickness (mm).

[0070] 4. The barium sulfate polymer composite material prepared in Example 1 was observed using a scanning electron microscope.

[0071] Results Analysis

[0072] Figure 1 This is a graph of the tensile strength test results of Examples 1-3 of the present invention and Comparative Examples 1-2. As shown in the figure, the tensile strengths of Examples 1-3 are 71 MPa, 72 MPa, and 70 MPa, respectively, while Comparative Example 1 is 52 MPa and Comparative Example 2 is 59 MPa. The tensile strengths of Examples 1-3 are significantly greater than those of Comparative Example 1, indicating that the modification of nano-barium sulfate enhances the tensile strength of the material. The tensile strengths of Examples 1-3 are significantly greater than those of Comparative Example 2, indicating that the addition of multi-walled carbon nanotubes and glass fibers enhances the tensile strength of the material.

[0073] Figure 2This is a graph of the compressive strength test results of Examples 1-3 of the present invention and Comparative Examples 1-2. As shown in the figure, the compressive strengths of Examples 1-3 are 89 MPa, 90 MPa, and 91 MPa, respectively, Comparative Example 1 is 61 MPa, and Comparative Example 2 is 67 MPa; the compressive strengths of Examples 1-3 are significantly greater than those of Comparative Example 1, indicating that the modification of nano-barium sulfate enhances the compressive strength of the material; the compressive strengths of Examples 1-3 are significantly greater than those of Comparative Example 2, indicating that the addition of multi-walled carbon nanotubes and glass fibers enhances the compressive strength of the material.

[0074] Figure 3 This is a graph of the bending strength test results of Examples 1-3 of the present invention and Comparative Examples 1-2. As shown in the figure, the bending strengths of Examples 1-3 are 92 MPa, 93 MPa, and 92 MPa, respectively, while Comparative Example 1 is 66 MPa and Comparative Example 2 is 71 MPa. The bending strengths of Examples 1-3 are significantly greater than those of Comparative Example 1, indicating that modification of nano-barium sulfate enhances the bending strength of the material. The bending strengths of Examples 1-3 are significantly greater than those of Comparative Example 2, indicating that the addition of multi-walled carbon nanotubes and glass fibers enhances the bending strength of the material.

[0075] Figure 4 This is a scanning electron microscope image of the barium sulfate polymer composite material prepared in Example 1 of the present invention.

[0076] While the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that many changes, modifications, substitutions and variations can be made to the embodiments without departing from the principles and spirit of the invention.

[0077] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A barium sulfate polymer composite material, characterized in that: The invention comprises the following components in parts by weight: 80-100 parts of epoxy resin, 10-20 parts of modified nano barium sulfate, 6-8 parts of multi-walled carbon nanotubes, 7-9 parts of glass fiber, 20-30 parts of acetone, and 10-15 parts of 4,4'-diaminodiphenylmethane curing agent; The preparation method of the modified nano barium sulfate comprises the following steps: (1) Add barium chloride and sodium sulfate to 100 mL of deionized water, stir to fully dissolve, then transfer to a flask, add oleic acid, heat to 80-90°C, stir at 600 rpm for 30-40 min, filter after completion, wash with deionized water 3 times, and vacuum dry at 50°C to obtain oleic acid-modified nano-barium sulfate; (2) Add the oleic acid-modified nano-barium sulfate obtained in step (1) into a flask, add methyl methacrylate, add divinylbenzene, and perform ultrasonic treatment for 10-20 min at a power of 400 W. Then, add initiator azobisisobutyronitrile, react at 60° C. and 400 rpm for 40-60 min. Take the precipitate, wash it with deionized water three times, then add it to 100 mL of methanol, add ethylenediamine, and react at 60° C. for 20-24 h to obtain ethylenediamine-modified nano-barium sulfate. (3) Add polyethyleneimine to methanol to obtain a polyethyleneimine solution, add the ethylenediamine-modified nano-barium sulfate obtained in step (1) to the polyethyleneimine solution, stir magnetically at room temperature for 20-24 hours at a stirring speed of 300-400 rpm, add 1 wt % glutaraldehyde aqueous solution, continue stirring for 30-40 minutes, and wash with deionized water three times to obtain modified nano-barium sulfate.

2. The barium sulfate polymer composite material according to claim 1, characterized in that: In step (1), the mass ratio of the barium chloride to the sodium sulfate is 1:2-3; in step (1), the volume ratio of the oleic acid to the deionized water is 1-2:

100.

3. The barium sulfate polymer composite material according to claim 2, characterized in that: In step (2), the volume ratio of divinylbenzene to methyl methacrylate is 1:15-20.

4. The barium sulfate polymer composite material according to claim 3, characterized in that: In step (2), the mass ratio of the oleic acid-modified nano-barium sulfate to azobisisobutyronitrile is 1:1-2.

5. The barium sulfate polymer composite material according to claim 4, characterized in that: In step (2), the mass ratio of the oleic acid-modified nano-barium sulfate to ethylenediamine is 1:2-4.

6. The barium sulfate polymer composite material according to claim 5, characterized in that: In step (3), the mass fraction of the polyethyleneimine in methanol is 2%-3%.

7. The barium sulfate polymer composite material according to claim 6, characterized in that: In step (3), the mass concentration of the ethylenediamine-modified nano-barium sulfate in the polyethyleneimine solution is 20-30 g / L.

8. The barium sulfate polymer composite material according to claim 7, characterized in that: In step (3), in step (3), the volume ratio of the glutaraldehyde aqueous solution to the polyethyleneimine solution is 3-4:

1.

9. The method for preparing a barium sulfate polymer composite material according to any one of claims 1 to 8, characterized in that: The method specifically comprises the following steps: adding multi-walled carbon nanotubes and glass fibers into acetone, stirring for 2-3 hours, then adding epoxy resin, continuing stirring for 3-4 hours, adding modified nano barium sulfate and 4,4'-diaminodiphenylmethane curing agent, stirring for 1-2 hours, and curing at room temperature for 10-20 hours to obtain a barium sulfate polymer composite material.