Non-platinum curing release agent, chemically stable release film and preparation method thereof

By using non-platinum curing release agent and visible light curing technology, gold nanoparticles are used to promote the hydrogen silicon addition reaction, and the problems of platinum catalyst toxicity and low release film stability are solved, and high-performance, chemically stable release film is prepared. , suitable for multi-field applications.

CN118389059BActive Publication Date: 2024-11-05YANGZHOU ALVIN OPTOELECTRONIC TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410852929.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-05
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

The use of platinum catalysts in existing photoinitiation curing methods leads to catalyst toxicity and product application limitations, and the release film has low chemical stability, which limits its application in biomedical, electronic and other fields.

Method used

Using non-platinum curing release agents, including silicones, sulfonic acid acrylic monomers, spherical gold nanoparticles, metal salts and initiators, chemically stable release films are prepared through visible light curing technology, and using gold nanoparticles to promote silicon hydrogen Addition polymerization reaction reduces side reactions.

Benefits of technology

It has achieved the avoidance of catalyst toxication and the reduction of by-products, and produced a release film with high selectivity, high temperature resistance, acid and alkali resistance, uniform surface, and low peeling force, meeting the application needs of food processing, pharmaceutical and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118389059B_ABST
    Figure CN118389059B_ABST
Patent Text Reader

Abstract

The invention discloses a non-platinum curing release agent, a chemically stable release film and a preparation method thereof, and belongs to the technical field of release materials. The non-platinum curing release agent is prepared from the following raw materials in parts by weight: 85 parts of siloxane; wherein the proportion of hexenyl polydimethylsiloxane is more than 80wt%, and the rest is hydrogen-containing siloxane; sulfonic acid acrylic monomer, (2-8) parts; photocatalyst, (0.1-1.2) parts; metal salt, (0.5-1.6) parts; initiator, (0.2-5) parts. The photocurable release agent is mixed evenly and then coated on a substrate, and photocured under visible light to obtain a release film. The gold nanoparticles used in the invention have the advantages of high catalytic activity and high selectivity. The introduced sulfonic acid acrylic monomer can regulate the surface properties of the release film, and enhance the chemical stability of the release film by complexing metal ions. The release film prepared by the invention has good chemical stability, uniformity, and low peeling force.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of release materials, and in particular to a non-platinum curing release agent, a chemically stable release film and a preparation method thereof. Background Art

[0002] Under certain conditions, hydrogen-containing siloxanes and siloxanes containing unsaturated bonds such as olefins and alkynes undergo hydrosilylation polymerization to generate elastic three-dimensional network materials with a certain cross-linking density. This is an effective method for producing organosilicon compounds and one of the most important reactions in silicon chemistry. Monomers with specific functions can be introduced and added to organosilicon compounds to provide the products with many unique and favorable properties. Various organosilicon products generated by hydrosilylation polymerization can be used in release films, lubricants, coatings, etc. To synthesize highly complex organosilicon materials for specific application scenarios, it is very important to develop catalysts with high selectivity, good compatibility and stability.

[0003] Platinum catalysts are widely used in the production of industrial release films due to their high catalytic activity and high stability. However, the platinum-catalyzed hydrosilylation of olefins is often accompanied by side reactions, such as dehydrogenative silylation, olefin hydrogenation, olefin isomerization, olefin oligomerization, and redistribution of hydrosilanes, which result in significant loss of product yield. In addition, the presence of by-products can also lead to release film contamination, requiring additional processes to remove, and will limit the application of release films in fields such as biomedicine or electronics. Therefore, it is of great significance to develop a catalyst with high efficiency and high selectivity to achieve a more economical production of release films with excellent performance.

[0004] In the method of preparing release film, the catalyst is mainly excited by light or heat to make the initiator produce free radicals, which ultimately promotes the hydrosilylation polymerization reaction. Among them, photocuring technology has the advantages of high reaction rate, solvent-free conditions, controllable ambient temperature, low energy consumption, simple equipment, etc., and is more environmentally friendly than thermal curing, and is the development direction of future industrial production. However, in the field of photocuring technology, the development of catalysts that respond efficiently to visible light (wavelength ≥ 420nm) is still a huge challenge. Visible light radiation is safer than ultraviolet light (wavelength < 420nm), has stronger chemical selectivity, fewer side reactions, and is also more environmentally friendly (low energy consumption, no release of ozone or harmful ultraviolet rays).

[0005] In addition, with the widespread application of release films in food processing, pharmaceutical, chemical industry and other fields, more stringent requirements are put forward on the strength, peeling force, high temperature resistance and chemical stability of release films. Therefore, the research and development of efficient and highly selective catalysts and suitable catalytic reaction systems are of great significance to the production of high-performance release films. Summary of the invention

[0006] In order to solve the problems of catalyst poisoning and limited product application caused by the use of platinum catalysts in existing photoinduced curing methods; and the problem of low chemical stability of existing release films, the present invention provides a non-platinum curing release agent, a chemically stable release film and a preparation method thereof.

[0007] The technical solution adopted by the present invention is:

[0008] A non-platinum curing release agent comprises the following raw materials in parts by weight:

[0009] Siloxane, 85 parts; of which hexenyl polydimethylsiloxane accounts for more than 80wt%, and the rest is hydrogen-containing siloxane;

[0010] Sulfonic acid acrylic monomer, (2–8) parts;

[0011] Photocatalyst, (0.1–1.2) parts;

[0012] Metal salt, (0.5–1.6) parts;

[0013] Initiator, (0.2–5) parts;

[0014] The photocatalyst is spherical gold nanoparticles.

[0015] The structural formula of hexenyl polydimethylsiloxane is:

[0016] R1 = vinyl or allyl, R2 = C 0–6 Hydrocarbyl, n is an integer from 10 to 1000;

[0017] The structural formula of hydrogen siloxane is:

[0018] R3=H or methyl, m is an integer from 10 to 1000.

[0019] Furthermore, the number average molecular weight of the siloxane is 250,000-700,000.

[0020] Furthermore, the initiator is at least one of ethyl α-bromophenylacetate, 2,4-diethylthioxanthone and 2-isopropylthioxanthone.

[0021] Furthermore, the diameter of the spherical gold nanoparticles is 25-80 nm.

[0022] Furthermore, the sulfonic acid acrylic acid monomer is 2-acrylamido-2-methyl-1-propane sulfonic acid and / or 3-sulfonate propyl potassium methacrylate.

[0023] Furthermore, the metal element in the metal salt is any one of Mn, Zn, Cu and Fe.

[0024] A chemically stable release film comprises a substrate and any one of the above-mentioned photocurable release agents coated on one side of the substrate.

[0025] Furthermore, the material of the substrate is PET, and the thickness of the release agent layer is 22-45 μm.

[0026] The method for preparing any one of the above release films comprises the following steps:

[0027] (1) Siloxane, sulfonic acid acrylic monomer, photocatalyst, initiator and metal salt are mixed according to a proportion and stirred evenly to obtain a release agent;

[0028] (2) The release agent prepared in step (1) is uniformly coated on the substrate in a certain thickness, and cured under irradiation of visible light to obtain a release film.

[0029] The reaction principle of light curing is as follows:

[0030]

[0031] Sulfonic acid acrylic monomers can adjust the hydrophilicity of the release film on the one hand, and on the other hand, can complex the added metal ions to enhance the stability of the release film. By controlling the ratio of the two siloxanes to the sulfonic acid acrylic monomers, that is, adjusting the ratio of x / y / z, the performance of the release film can be adjusted.

[0032] Furthermore, the wavelength of visible light is ≥420 nm, the ambient temperature of the curing reaction is 5–45° C., and the reaction time is 1–12 hours.

[0033] Beneficial effects of the present invention:

[0034] 1. Gold is a chemically inert element, but at the nanoscale, it exhibits outstanding and unique properties. Gold is easy to synthesize, has good biocompatibility, is easy to size-control, and has adjustable optical properties. These properties make it widely used in various fields, especially in the field of photocatalysis. Under visible light conditions, the surface plasma of gold nanoparticles is excited and enters an excited state, generating localized surface plasmon resonance (LSPR). J. Am. Chem. Soc. 2011, 133,595–602), the excited state can promote the initiator to produce free radicals, thereby promoting the reaction. The present invention uses visible light to excite the catalyst gold nanoparticles to reach an excited state, so that the initiator produces free radicals, significantly promotes the hydrosilylation polymerization reaction, and quickly prepares the release film without catalyst poisoning and residual byproducts.

[0035] 2. The present invention can adjust the hydrophilicity of the release film by introducing sulfonic acid acrylic monomers, and can complex the added metal ions, and the addition of metal ions can enhance the stability of the release film. In addition, after the sulfonic acid acrylic monomers are introduced, the chemical stability of the release film is improved due to the interaction of van der Waals force and hydrogen bond, and the surface smoothness of the release film is contributed to a certain extent, and the release film has good adaptability to use in special environments.

[0036] 3. The present invention uses visible light curing technology to prepare the release film, the reaction conditions are safer and more environmentally friendly, and the process is controllable.

[0037] In general, the present invention uses gold nanoparticle catalysts and visible light curing methods to prepare release films, which has the advantages of simple operation, strong selectivity, safe and environmentally friendly processes, etc., and can produce release films with excellent performance in a more economical way. The produced release films have the characteristics of high temperature resistance, acid and alkali resistance, uniform surface, low and controllable peeling force, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a transmission electron microscopy image of the gold nanoparticles used in Example 1.

[0039] Figure 2 This is the UV-visible absorption spectrum of the gold nanoparticles used in Example 1.

[0040] Figure 3 This is an infrared spectrum of the release film A prepared in Example 1 before and after photocuring.

[0041] Figure 4 This is the hydrogen nuclear magnetic resonance spectrum of the release film A prepared in Example 1 before and after photocuring.

[0042] Figure 5 This is a 3D height map of the release film A prepared in Example 1.

[0043] Figure 6 This is the infrared spectrum of the release film A prepared in Example 1 before and after acid and alkali treatment.

[0044] Figure 7 This is the hydrogen nuclear magnetic resonance spectrum of the release film A prepared in Example 1 before and after acid-base treatment.

[0045] Figure 8 The thermal analysis data of the release films prepared in Example 1 and Comparative Example 2 are shown in FIG. DETAILED DESCRIPTION

[0046] The technical solution of the present invention is described in detail below through specific embodiments, but the protection scope of the present invention is not limited to the embodiments.

[0047] The raw materials used in the following examples and comparative examples are all commercially available.

[0048] Hexenyl polydimethylsiloxane was purchased from Dow Corning Corporation of the United States. The product models with number average molecular weights of approximately 500,000 and 700,000 were PC183-50 and PC183-70, respectively, and were used after removing the solvent.

[0049] Hydrogen-containing siloxane was purchased from Dow Corning (HH127) and was used after removing the solvent.

[0050] Photocatalyst: Gold nanoparticles were purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd. The gold nanoparticles with a diameter of 50 nm are model XFJ60-1104098, and the gold nanoparticles with a diameter of 80 nm are model XFJ60-1104264.

[0051] Sulfonic acid acrylic monomers: 2-acrylamido-2-methyl-1-propane sulfonic acid (A800508) and potassium 3-sulfonate propyl methacrylate (S817739) were purchased from MacLean Company.

[0052] Initiator: α-bromophenylacetate (A76604) was purchased from Beijing Inokai Co., Ltd., 2,4-diethylthioxanthone (D837902) and 2-isopropylthioxanthone (I834922) were purchased from MacLean Company.

[0053] Metal salts: anhydrous zinc chloride (A30488), ferrous chloride (A82336), manganese chloride (A94486), and cupric chloride (A20337) were purchased from Beijing Inokai Co., Ltd. Example 1

[0054] The preparation method of the light-curing release film A is as follows:

[0055] (1) 8.2 g of hexenyl polydimethylsiloxane with a number average molecular weight of about 500,000 and 1.8 g of hydrogen-containing siloxane were mixed evenly, and 0.8 g of 2-acrylamido-2-methyl-1-propane sulfonic acid, 1 ml of photocatalyst gold nanoparticles (diameter 50 nm, 100 mg / ml), 0.12 g of initiator 2,4-diethylthioxanthone, and 0.1 g of anhydrous zinc chloride were added, and the above components were mixed evenly to obtain a release agent A;

[0056] (2) The release agent A is uniformly coated on the surface of the PET substrate layer, and irradiated with visible light (wavelength = 550 nm) at a temperature of 20°C for a reaction time of 3 hours to obtain a photocurable release film A, wherein the thickness of the release agent layer is 25±2 μm.

[0057] The transmission electron microscopy and UV-visible absorption spectra of the gold nanoparticles used in this example are shown in Figure 1 and Figure 2 .from Figure 2It can be seen that gold nanoparticles have good absorption properties in the visible light range.

[0058] The light-curing release film A was characterized, and the results of infrared testing are shown in Figure 3 , H NMR spectrum analysis see Figure 4 .

[0059] from Figure 3 It can be found that after photocatalysis, the 2167cm- -1 The infrared absorption band at 1631 cm-1 is significantly weakened, and the 1631 cm-1 absorption band unique to olefins in the hexene group is -1 The infrared absorption band at the position disappears, indicating that the curing reaction has occurred. Figure 4 It can be found that after photocuring, a new chemical shift appeared at 3.44 ppm, corresponding to the methylene proton (-CH2-CH2-), proving the occurrence of the curing reaction.

[0060] The surface morphology of the prepared light-curable release film A was analyzed. Figure 5 ;from Figure 5 It can be found that the prepared release film has a uniform surface thickness and no obvious protrusions.

[0061] The prepared photocurable release film A was subjected to an acid-base stability test. The test method was as follows: the release film was immersed in a 0.1M hydrochloric acid solution and a 0.1M sodium hydroxide solution for 24 hours, then taken out and washed with deionized water, and then subjected to infrared and nuclear magnetic resonance tests. The test results are shown in FIG. Figure 6 and Figure 7 .from Figure 6 and Figure 7 It can be found that after being soaked in acid / alkaline, the characteristic peaks of the release film have no obvious changes, indicating that the prepared release film has good acid and alkali resistance. Example 2

[0062] The preparation method of the light-curing release film B is as follows:

[0063] (1) 8.2 g of hexenyl polydimethylsiloxane with a number average molecular weight of about 500,000 and 1.8 g of hydrogen-containing siloxane were mixed evenly, and 0.8 g of 2-acrylamido-2-methyl-1-propane sulfonic acid, 1 ml of photocatalyst gold nanoparticles (diameter 50 nm, 100 mg / ml), 0.12 g of initiator 2,4-diethylthioxanthone, and 0.1 g of ferrous chloride were added, and the above components were mixed evenly to obtain a release agent B;

[0064] (2) The release agent B is evenly coated on the surface of the PET substrate layer and irradiated with visible light (wavelength = 550 nm) at a temperature of 20°C for a reaction time of 3 hours to obtain a photocurable release film B, the thickness of which is 25±2 μm. Example 3

[0065] The preparation method of the light-curing release film C is as follows:

[0066] (1) 8.2 g of hexenyl polydimethylsiloxane with a number average molecular weight of about 500,000 and 1.8 g of hydrogen-containing siloxane were mixed evenly, and 0.8 g of potassium 3-sulfonate propyl methacrylate, 1 ml of photocatalyst gold nanoparticles (diameter 50 nm, 100 mg / ml), 0.15 g of initiator 2,4-diethylthioxanthone, and 0.1 g of anhydrous zinc chloride were added, and the above components were mixed evenly to obtain a release agent C;

[0067] (2) The release agent C was uniformly coated on the surface of the PET substrate layer and irradiated with visible light (wavelength = 550 nm) at a temperature of 20°C for a reaction time of 3 hours to obtain a photocurable release film C, the thickness of which was 38±2 μm. Example 4

[0068] The preparation method of the light-curing release film D is as follows:

[0069] (1) 8.2 g of hexenyl polydimethylsiloxane with a number average molecular weight of about 700,000 and 1.8 g of hydrogen-containing siloxane were mixed evenly, and 0.5 g of 2-acrylamido-2-methyl-1-propane sulfonic acid, 1.35 ml of photocatalyst gold nanoparticles (diameter 50 nm, 100 mg / ml), 0.12 g of initiator 2-isopropylthioxanthone, and 0.1 g of anhydrous zinc chloride were added, and the above components were mixed evenly to obtain a release agent D;

[0070] (2) The release agent D was uniformly coated on the surface of the PET substrate layer and irradiated with visible light (wavelength = 600 nm) at a temperature of 20°C for 4 hours to obtain a photocurable release film D, the thickness of which was 35±2 μm. Example 5

[0071] The preparation method of the light-curing release film E is as follows:

[0072] (1) 9.2 g of hexenyl polydimethylsiloxane with a number average molecular weight of about 700,000 and 0.8 g of hydrogen-containing siloxane were mixed evenly, and 0.8 g of 2-acrylamido-2-methyl-1-propane sulfonic acid, 1.0 ml of photocatalyst gold nanoparticles (diameter 80 nm, 100 mg / ml), 150 mg of initiator 2,4-diethylthioxanthone, and 0.15 g of anhydrous cupric chloride were added, and the above components were mixed evenly to obtain a release agent E;

[0073] (2) The release agent E was uniformly coated on the surface of the PET substrate layer and irradiated with visible light (wavelength = 600 nm) at a temperature of 20°C for a reaction time of 5 hours to obtain a photocurable release film E, wherein the thickness of the release agent layer was 38±2 μm. Example 6

[0074] The preparation method of the light-curing release film F is as follows:

[0075] (1) 9.2 g of hexenyl polydimethylsiloxane with a number average molecular weight of about 700,000 and 0.8 g of hydrogen-containing siloxane were mixed evenly, and 0.5 g of 2-acrylamido-2-methyl-1-propane sulfonic acid, 1.4 ml of photocatalyst gold nanoparticles (diameter 80 nm, 100 mg / ml), 0.12 g of initiator ethyl α-bromophenylacetate, and 0.15 g of anhydrous manganese chloride were added, and the above components were mixed evenly to obtain a release agent F;

[0076] (2) The release agent F was uniformly coated on the surface of the PET substrate layer and irradiated with visible light (wavelength = 600 nm) at a temperature of 20°C for a reaction time of 5 hours to obtain a photocurable release film E, wherein the thickness of the release agent layer was 38±2 μm.

[0077] Comparative Example 1

[0078] Comparative Example 1 is based on Example 1, except that no catalyst is added to the release agent.

[0079] Comparative Example 2

[0080] Comparative Example 2 is based on Example 1, except that no metal salt is added to the release agent.

[0081] The release films prepared in Example 1 and Comparative Example 2 were subjected to thermogravimetric analysis tests, and the results are shown in Figure 8 . Figure 8 It shows that after adding metal salts, the decomposition temperature of the release film is higher and the residual mass is more, indicating that the stability of the release film is significantly improved.

[0082] Comparative Example 3

[0083] Comparative Example 3 is based on Example 1, except that no sulfonic acid acrylic monomer is added to the release agent.

[0084] Thermal analysis tests were performed on the release films prepared in Example 1 and Comparative Example 2. The results are shown in Figure 8 ,from Figure 8 It can be seen that the metal ions added in the present invention have a significant effect on improving the stability of the release film.

[0085] The photocurable release films obtained in Examples 1-6 and Comparative Examples 1-3 were subjected to peel force tests, and the water contact angle and thickness range tests were performed on Examples 1-6 and Comparative Examples 2-3. The results are shown in Table 1. The peel force test adopts the standard: GB / T25256-2010; the thickness test adopts the standard: ASTM D882-18-2018.

[0086]

[0087] It can be seen from Table 1 that from the roughness results, the thickness distribution of the release film provided by the present invention is uniform.

[0088] From the comparison results of Examples 1-6 and Comparative Example 2, it can be seen that the addition of metal ions has a slight effect on the peeling force, while the type of ions has little effect on the peeling force and hydrophobicity.

[0089] From the comparison results of Examples 1-6, it can be seen that the size of the gold nanoparticles used in the present invention has a certain influence on the peeling force of the release film. The peeling force obtained by using gold nanoparticles with a diameter of about 50nm (Examples 1-4) is lower. The reasons are analyzed as follows: on the one hand, gold nanoparticles of different sizes have different excitation degrees, which affects the performance of the product; on the other hand, the gold nanoparticles left in the release film will also have a certain influence on the performance of the release film. Therefore, the peeling force can be fine-tuned by using gold nanoparticles of different sizes. At the same time, combined with the results of Comparative Example 3, it can be seen that the presence of sulfonic acid acrylic monomers has an effect on the peeling force, but the type of sulfonic acid acrylic monomers has little effect on the peeling force performance. In addition, the use of different proportions of siloxane also has an effect on the peeling force of the release film.

[0090] The water contact angle results of the release films obtained by comparing Examples 1-6 and Comparative Example 3 show that the sulfonic acid acrylic monomer introduced in the present invention can improve the hydrophilicity of the release film. The performance of the release films obtained by comparing Examples 1-6 and Comparative Example 1-3 show that the sulfonic acid acrylic monomer complexes the metal ions and improves the stability of the release film.

[0091] Combined with the above analysis, it can be seen that the ratio of the two siloxanes to the sulfonic acid acrylic monomers, the size of the catalyst, etc. will affect the performance of the release film, and it is a comprehensive process. In general, the release film provided by the present invention has a controllable and low peeling force and good chemical stability, meeting the requirements of food processing, pharmaceutical, chemical industry and other fields.

[0092] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A non-platinum curing release agent, It is characterized in that The following raw materials are used: composition: Siloxane, 85 parts; of which hexenyl polydimethylsiloxane accounts for more than 80wt%, and the rest is hydrogen-containing siloxane; Sulfonic acid acrylic monomer, (2–8) parts; Photocatalyst, (0.1–1.2) parts; Metal salt, (0.5–1.6) parts; Initiator, (0.2–5) parts; The photocatalyst is spherical gold nanoparticles; The number average molecular weight of the siloxane is 250,000-700,000; The initiator is at least one of ethyl α-bromophenylacetate, 2,4-diethylthioxanthone and 2-isopropylthioxanthone; The diameter of the spherical gold nanoparticles is 25–80 nm; The sulfonic acid acrylic acid monomer is 2-acrylamido-2-methyl-1-propane sulfonic acid or / and 3-sulfonate propyl methacrylate potassium; The metal element in the metal salt is any one of Mn, Zn, Cu and Fe.

2. A chemically stable release film, It is characterized in that The invention comprises a substrate and a non-platinum curing release agent as claimed in claim 1 coated on one side of the substrate.

3. A chemically stable release film according to claim 2, It is characterized in that The material of the substrate is PET, and the thickness of the release agent layer is 22–45 μm.

4. The method for preparing a chemically stable release film according to claim 2, It is characterized in that The following steps are involved: (1) Siloxane, sulfonic acid acrylic monomer, photocatalyst, initiator and metal salt are mixed according to a proportion and stirred evenly to obtain a release agent; (2) The release agent prepared in step (1) is uniformly coated on the substrate in a certain thickness, and cured under irradiation of visible light to obtain a release film.

5. The preparation method according to claim 4, It is characterized in that The wavelength of visible light is ≥420nm, the ambient temperature of the curing reaction is 5–45°C, and the reaction time is 1–12 hours.

Citation Information

Cited By

  • Photocuring silicon-based release agent and preparation method of PET release film

    CN121293872A

  • Preparation method of light-cured silicon-based release agent and PET release film

    CN121293872B