A bio-coal production process and its products and applications
By preparing biocoal crystals and modified agricultural waste, combined with specific binders and surfactants, the problem of insufficient thermal stability and transportation stability of biomass molded particles is solved, and high combustion efficiency and thermal value are achieved. Biocoal is suitable for high-efficiency and low-pollution combustion of large-scale power generation.
Patent Information
- Application Number
- CN202410648825.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-05-23
AI Technical Summary
Existing biomass molded particles are prone to looseness during long-term storage and have poor thermal stability, which affects their efficient and low-pollution combustion during large-scale power generation, increasing storage space requirements and crushing rate during transportation.
By preparing biocoal crystals and modified agricultural waste, combined with specific binders and surfactants, we form biocoal with high combustion efficiency and thermal stability, including biocoal crystals, domestic sludge, corn cobs, modified Agricultural waste, surfactants and binders are used to improve their thermal stability and transportation stability through sintering and composting processes.
It improves the thermal stability and transportation stability of biocoal, enhances combustion efficiency and thermal power value, reduces the ash content, and ensures the safety and efficiency of biocoal application in the energy industry.
Smart Images

Figure BDA0004855665950000101 
Figure BDA0004855665950000111
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of bio-coal, and in particular relates to a bio-coal production process and a product and application thereof. Background Art
[0002] Biomass refers to all plant and animal tissues on Earth that grow through photosynthesis, as well as the residues derived from these organisms, such as crop residues, wood waste, animal feces, algae, energy crops, etc. These organic substances contain chemical energy converted from solar energy, which is biomass energy. Biomass energy is an important part of the renewable energy family. It can provide a diversified source of energy and reduce excessive dependence on fossil fuels (such as coal, oil, and natural gas), thereby improving the security and stability of energy supply. As a renewable resource, biomass is of great significance in ensuring energy security, mitigating climate change, promoting a circular economy, promoting social and economic development, and protecting the ecology.
[0003] Biomass itself has the characteristics of large volume, light weight, easy to ignite, wide distribution area, and seasonal harvesting. In order to facilitate biomass collection, transportation and storage, biomass molding compression technology is usually used to make biomass molded fuel. However, the biomass molded particles at home and abroad are easy to loosen and have poor thermal stability when stored for a long time. When directly used for power generation on a large scale, the storage space demand is increased, and the breakage rate during transportation is increased, which affects the continuous and stable feeding and cannot achieve efficient and low-pollution combustion. Summary of the invention
[0004] The purpose of the present invention is to provide a production process of bio-coal and its products and applications, wherein the bio-coal has high thermal stability and transportation stability, and also has high combustion efficiency and thermal value.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] A bio-coal comprising the following raw materials in parts by weight: 16 to 20 parts of bio-coal crystals, 10 to 14 parts of domestic sludge, 3 to 7 parts of corn cobs, 18 to 22 parts of modified agricultural waste, 0.4 to 0.8 parts of a surfactant, 20 to 24 parts of a binder and 120 to 130 parts of water;
[0007] The preparation method of the bio-coal crystals is as follows: the cotton stalks are crushed into 1-2 cm, placed in a closed sintering furnace, heated to 500-700° C. under negative atmospheric pressure, kept warm for 6-9 hours, the sintering furnace stops heating and maintains negative pressure, cooled and crystallized to obtain bio-coal crystals;
[0008] The preparation method of the modified agricultural waste is:
[0009] (1) Cotton straw, peanut skin and corn straw are crushed respectively and particles with a particle size of 60 to 100 mesh are selected, and the cotton straw, peanut skin and corn straw particles are mixed in a weight ratio of 2 to 3:1:0.3 to 0.8 to obtain mixed agricultural waste.
[0010] (2) immersing the crushed biomass particles in a sodium hydroxide aqueous solution having a mass fraction of 10 to 12%, heating the mixture to 80 to 90° C., and steaming the mixture for 140 to 160 minutes; filtering the mixture, and washing the mixture with water until the mixture is neutral to obtain alkalized agricultural waste;
[0011] (3) adding water to the alkalized agricultural waste to make its moisture content 62-65wt%, adding a decomposing bacteria agent, and performing aerobic ventilated composting at a composting height of 1.3-1.6m. When the temperature of the pile body rises to 60-65°C, it is maintained for 8-10 days and the pile is turned; when the temperature rises to 50-55°C, it is maintained for 6-8 days, and the composting is completed; and drying is performed to obtain modified agricultural waste with a moisture content of 40-45%.
[0012] Furthermore, the decomposing bacteria agent is a compound of amylase, brewer's yeast and protease in a weight ratio of 1.3-1.5:1:0.4-0.7.
[0013] Furthermore, the amount of the decomposing bacteria agent added is 0.2 to 0.4% of the weight of the alkalized agricultural waste.
[0014] Furthermore, amylase, Shanghai Yuanye Biotechnology Co., Ltd., product number S68733; Saccharomyces cerevisiae, Shanghai Yuanye Biotechnology Co., Ltd., product number Y41643; protease, Shanghai Yuanye Biotechnology Co., Ltd., product number: S10051.
[0015] Cotton stalks, peanut skins and corn stalks are commonly used raw materials for biomass fuels, and recycling them has extremely high environmental value. In the prior art, they are crushed and directly used to make bio-coal, but the combustion efficiency is not ideal. The present invention pre-treats cotton stalks, peanut skins and corn stalks, sinters the cotton stalks and turns them into crystals to obtain bio-coal crystals, and compound the bio-coal crystals, domestic sludge and corn cobs in a specific proportion to improve the combustion efficiency of the bio-coal. Analysis shows that alkalization can make the structure more fluffy and open, and the original tight network structure is destroyed, while changing the composition of the ash. Further fermentation by composting bacteria changes the functional groups inside the waste, improves the activation energy, is conducive to pyrolysis, and provides better thermal efficiency.
[0016] Furthermore, the preparation method of the binder comprises the following steps:
[0017] (1) Mix 1 part by weight of starch and 3 to 5 parts by weight of water, raise the temperature to 36° C. to 37° C., add 0.05 to 0.07 parts by weight of sodium chloride and 0.2 to 0.3 parts by weight of sodium hypochlorite, react for 6 to 8 hours, adjust the pH to 11.2 to 11.5, then add 0.1 to 0.15 parts by weight of sodium chloride and 0.2 to 0.25 parts by weight of propylene oxide in sequence, react at 36° C. to 37° C. for 25 to 30 hours, adjust the pH to neutral, and filter to obtain modified starch;
[0018] (2) Diatomaceous earth, emulsified asphalt and modified starch are mixed in a weight ratio of 0.5 to 0.8:1:1.2 to 1.5 and stirred evenly to obtain a binder.
[0019] Furthermore, the diatomite particle size is, with a specific surface area of 20m 2 / g~30m 2 / g, and the pore radius is 100nm-200nm.
[0020] Furthermore, the emulsified asphalt is from Shak (Tianjin) Petroleum Technology Service Co., Ltd. Emulsified asphalt.
[0021] The biocoal binders on the market mainly include inorganic binders and organic binders. Inorganic binders are low in price and good in thermal stability, but have poor bonding properties and increase ash content; most organic binders have good bonding properties and a certain calorific value, but have poor thermal stability and are expensive. The use effect of adding commercially available binders to the system of the present invention is not ideal. The binder of the present invention is compounded by multiple components to modify starch to obtain hydroxypropyl modified starch, and synergizes with diatomaceous earth and emulsified asphalt to improve the anti-drop ability and improve the transportation stability of biocoal. The inventors found that the use of specific diatomaceous earth and emulsified asphalt can improve the thermal stability of biocoal. The analysis shows that the binder of the present invention has better compatibility with the raw materials in the system, and can form a stronger and tougher bonding interface with biocoal crystals, domestic sludge, corn cobs, and modified agricultural waste, and the bonding force is stronger. At the same time, the present invention uses specific diatomaceous earth, emulsified asphalt and surfactants to improve the thermal stability of biocoal. Analysis Emulsified asphalt is a product based on high-quality natural asphalt. The surface of asphalt particles is modified using a special process so that the surface of the particles has a positive charge, which can evenly wrap the biocoal particles, strengthen the connection between the particles, form a dense structure, and reduce the gaps between the particles, thereby improving thermal stability. Diatomaceous earth with a specific structure can be embedded in the gaps between biocoal particles due to its special microscopic pore structure and large specific surface area, increasing the density and strength of the coal body and reducing structural fractures caused by stress changes during combustion. Surfactants improve the dispersibility of the system components and enhance the stability of the cross-linked structure.
[0022] Furthermore, the surfactant is a compound of sodium dodecylbenzene sulfonate (CAS: 25155-30-0), hexadecyltrimethylammonium chloride (CAS: 112-02-7) and fatty alcohol polyoxyethylene ether (AEO-9) in a weight ratio of 1:1.5-1.7:0.2-0.5.
[0023] Further, the water content of the domestic sludge is less than 75%.
[0024] The present invention also provides a production process of the bio-coal, comprising the following steps:
[0025] Step 1: Add bio-coal crystals, domestic sludge, corn cobs, modified agricultural waste, surfactants, binders and water into a kneader, knead evenly, and ripen for 3 to 4 hours to obtain a mixed material;
[0026] Step 2: Press the mixed material into a shape, first dry it at 50-55° C. for 150-170 min, then dry it at 110-115° C. for 80-100 min, and obtain biocoal after cooling.
[0027] The third aspect of the present invention provides the application of the bio-coal in the energy industry.
[0028] Compared with the prior art, the advantages and beneficial effects of the present invention are:
[0029] 1. The present invention provides a bio-coal production process and its products and applications. The bio-coal has high thermal stability and transportation stability, as well as high combustion efficiency and thermal value.
[0030] 2. The present invention improves the combustion efficiency of bio-coal by pre-treating cotton stalks, peanut skins and corn stalks and compounding them with bio-coal crystals, domestic sludge and corn cobs in a specific proportion.
[0031] 3. The binder of the present invention is prepared by compounding multiple components to modify starch to obtain hydroxypropyl modified starch, and works synergistically with diatomaceous earth and emulsified asphalt to enhance the anti-drop ability and improve the transportation stability of bio-coal.
[0032] 4. The present invention uses specific diatomaceous earth, emulsified asphalt and surfactant to improve the thermal stability of bio-coal. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Example 1
[0035] This embodiment provides a bio-coal, comprising the following raw materials in parts by weight: 18 parts of bio-coal crystals, 12 parts of domestic sludge, 5 parts of corn cobs, 21 parts of modified agricultural waste, 0.6 parts of surfactant, 22 parts of binder and 125 parts of water;
[0036] The preparation method of the bio-coal crystals is as follows: the cotton stalks are crushed into 1-2 cm, placed in a closed sintering furnace, heated to 600° C. under negative atmospheric pressure, kept warm for 8 hours, the sintering furnace stops heating and maintains negative pressure, cooled and crystallized to obtain bio-coal crystals;
[0037] The preparation method of the modified agricultural waste is:
[0038] (1) crushing cotton straw, peanut skin and corn straw respectively and selecting particles with a particle size between 60 and 100 meshes, and then mixing the cotton straw, peanut skin and corn straw particles in a weight ratio of 2.5:1:0.6 to obtain mixed agricultural waste;
[0039] (2) immersing the crushed biomass particles in an aqueous sodium hydroxide solution having a mass fraction of 11%, heating the mixture to 85° C., and steaming the mixture for 150 minutes; filtering the mixture, and washing the mixture with water until the mixture is neutral, thereby obtaining alkalized agricultural waste;
[0040] (3) adding water to the alkalized agricultural waste to make its moisture content 64wt%, adding a decomposing bacteria agent, and carrying out aerobic ventilated composting with a composting height of 1.5m. When the temperature of the pile body rises to 63°C, it is maintained for 9 days and the pile is turned; when the temperature rises to 53°C, it is maintained for 7 days, and the composting is completed; and drying is carried out to obtain modified agricultural waste with a moisture content of 43%.
[0041] The decomposing bacteria agent is a compound of amylase, brewer's yeast and protease in a weight ratio of 1.4:1:0.6.
[0042] The amount of the decomposing bacteria agent added is 0.3% of the weight of the alkalized agricultural waste.
[0043] Amylase, Shanghai Yuanye Biotechnology Co., Ltd., product number S68733; Saccharomyces cerevisiae, Shanghai Yuanye Biotechnology Co., Ltd., product number Y41643; Protease, Shanghai Yuanye Biotechnology Co., Ltd., product number: S10051.
[0044] The preparation method of the binder comprises the following steps:
[0045] (1) 1 part by weight of starch and 4 parts by weight of water were mixed, the temperature was raised to 36° C., 0.06 parts by weight of sodium chloride and 0.2 parts of sodium hypochlorite were added, the reaction was continued for 7 hours, the pH value was adjusted to 11.4, and 0.12 parts by weight of sodium chloride and 0.22 parts by weight of propylene oxide were added in sequence, the reaction was continued at 36° C. for 28 hours, the pH value was adjusted to neutral, and the mixture was filtered to obtain modified starch;
[0046] (2) Diatomaceous earth, emulsified asphalt and modified starch in a weight ratio of 0.7:1:1.3 are mixed and stirred evenly to obtain a binder.
[0047] The diatomite particle size is, with a specific surface area of 20m 2 / g~30m 2 / g, and the pore radius is 100nm-200nm.
[0048] The emulsified asphalt is from Shak (Tianjin) Petroleum Technology Service Co., Ltd. Emulsified asphalt.
[0049] The surfactant is a compound of sodium dodecylbenzene sulfonate (CAS: 25155-30-0), hexadecyltrimethylammonium chloride (CAS: 112-02-7) and fatty alcohol polyoxyethylene ether (AEO-9) in a weight ratio of 1:1.6:0.3.
[0050] The water content of domestic sludge is less than 75%.
[0051] The bio-coal production process comprises the following steps:
[0052] Step 1: Add bio-coal crystals, domestic sludge, corn cobs, modified agricultural waste, surfactants, binders and water into a kneader, knead evenly, and ripen for 3.5 hours to obtain a mixed material;
[0053] Step 2: Press the mixed material into a shape, first dry it at 52° C. for 160 min, then dry it at 112° C. for 90 min, and obtain biocoal after cooling.
[0054] Example 2
[0055] This embodiment provides a bio-coal, comprising the following raw materials in parts by weight: 20 parts of bio-coal crystals, 10 parts of domestic sludge, 7 parts of corn cobs, 18 parts of modified agricultural waste, 0.8 parts of surfactant, 20 parts of binder and 130 parts of water;
[0056] The preparation method of the bio-coal crystals is as follows: the cotton stalks are crushed into 1-2 cm, placed in a closed sintering furnace, heated to 700°C under negative atmospheric pressure, kept warm for 6 hours, the sintering furnace stops heating and maintains negative pressure, cooled and crystallized to obtain bio-coal crystals;
[0057] The preparation method of the modified agricultural waste is:
[0058] (1) crushing cotton straw, peanut skin and corn straw respectively and selecting particles with a particle size between 60 and 100 meshes, and then mixing the cotton straw, peanut skin and corn straw particles in a weight ratio of 2:1:0.8 to obtain mixed agricultural waste;
[0059] (2) immersing the crushed biomass particles in a 12% by mass sodium hydroxide aqueous solution, heating to 80° C., and steaming for 160 minutes; filtering and washing with water until neutral to obtain alkalized agricultural waste;
[0060] (3) adding water to the alkalized agricultural waste to make its moisture content 62wt%, adding a decomposing bacteria agent, and conducting aerobic ventilated composting with a composting height of 1.6m. When the temperature of the pile body rises to 60°C, it is maintained for 10 days and the pile is turned; when the temperature rises to 50°C, it is maintained for 8 days, and the composting is completed; and drying is performed to obtain modified agricultural waste with a moisture content of 40%.
[0061] The decomposing bacteria agent is a compound of amylase, brewer's yeast and protease in a weight ratio of 1.5:1:0.4.
[0062] The amount of the decomposing bacteria agent added is 0.4% of the weight of the alkalized agricultural waste.
[0063] Amylase, Shanghai Yuanye Biotechnology Co., Ltd., product number S68733; Saccharomyces cerevisiae, Shanghai Yuanye Biotechnology Co., Ltd., product number Y41643; Protease, Shanghai Yuanye Biotechnology Co., Ltd., product number: S10051.
[0064] The preparation method of the binder comprises the following steps:
[0065] (1) 1 part by weight of starch and 3 parts by weight of water were mixed, the temperature was raised to 37° C., 0.05 parts by weight of sodium chloride and 0.3 parts of sodium hypochlorite were added, the reaction was continued for 6 hours, the pH was adjusted to 11.5, and 0.1 parts by weight of sodium chloride and 0.25 parts by weight of propylene oxide were added in sequence, the reaction was continued at 37° C. for 30 hours, the pH was adjusted to neutral, and the mixture was filtered to obtain modified starch;
[0066] (2) Diatomaceous earth, emulsified asphalt and modified starch in a weight ratio of 0.5:1:1.5 are mixed and stirred evenly to obtain a binder.
[0067] The diatomite particle size is, with a specific surface area of 20m 2 / g~30m 2 / g, and the pore radius is 100nm-200nm.
[0068] The emulsified asphalt is from Shak (Tianjin) Petroleum Technology Service Co., Ltd. Emulsified asphalt.
[0069] The surfactant is a compound of sodium dodecylbenzene sulfonate (CAS: 25155-30-0), hexadecyltrimethylammonium chloride (CAS: 112-02-7) and fatty alcohol polyoxyethylene ether (AEO-9) in a weight ratio of 1:1.5:0.5.
[0070] The water content of domestic sludge is less than 75%.
[0071] The bio-coal production process comprises the following steps:
[0072] Step 1: Add bio-coal crystals, domestic sludge, corn cobs, modified agricultural waste, surfactants, binders and water into a kneader, knead evenly, and ripen for 3 hours to obtain a mixed material;
[0073] Step 2: Press the mixed material into a shape, first dry it at 50°C for 170 minutes, then dry it at 110°C for 100 minutes, and obtain biocoal after cooling.
[0074] Comparative Example 1
[0075] The difference between this comparative example and Example 1 is: a bio-coal comprising the following raw materials in parts by weight: 13 parts of bio-coal crystals, 17 parts of domestic sludge, 10 parts of corn cobs, 16 parts of modified agricultural waste, 0.6 parts of surfactant, 22 parts of binder and 125 parts of water.
[0076] Comparative Example 2
[0077] The difference between this comparative example and Example 1 is that the modified agricultural waste is replaced by agricultural waste.
[0078] A bio-coal comprises the following raw materials in parts by weight: 18 parts of bio-coal crystals, 12 parts of domestic sludge, 5 parts of corn cobs, 21 parts of agricultural waste, 0.6 parts of surfactant, 22 parts of binder and 125 parts of water. The agricultural waste is a mixture of cotton stalks, peanut skins and corn stalks with a weight ratio of 2.5:1:0.6 and particles with a particle size of 60 to 100 meshes.
[0079] Comparative Example 3
[0080] The difference between this comparative example and Example 1 is that the decomposing bacteria agent is a compound of amylase, saccharomyces cerevisiae and protease in a weight ratio of 1:1:1.
[0081] Comparative Example 4
[0082] The difference between this comparative example and Example 1 is that the decomposition bacteria agent is a compound of Bacillus subtilis (Weifang Yihao Biotechnology Co., Ltd., 50 U / mg), thermophilic Bacillus (Hunan Fenghui Biotechnology Co., Ltd., 50 U / mg) and protease (Shanghai Yuanye Biotechnology Co., Ltd., product number: S10051) in a weight ratio of 1.4:1:0.6.
[0083] Comparative Example 5
[0084] The difference between this comparative example and Example 1 is that the binder is an organic binder: sodium humate (Shenyang Elex Chemical Co., Ltd.).
[0085] Comparative Example 6
[0086] The difference between this comparative example and Example 1 is that the preparation method of the binder comprises the following steps: diatomaceous earth, emulsified asphalt and starch in a weight ratio of 1:1:1 are mixed and stirred evenly to obtain a binder.
[0087] Comparative Example 7
[0088] The difference between this comparative example and Example 1 is:
[0089] The diatomite particle size is, with a specific surface area of 5m 2 / g~10m 2 / g, and the pore radius is 30nm-70nm.
[0090] The emulsified asphalt comes from Hebei Dezhishan Petrochemical Co., Ltd., model 90.
[0091] The surfactant is a compound of octadecyl dimethyl benzyl ammonium chloride (CAS: 122-19-0), Tween-60 and fatty alcohol polyoxyethylene ether (AEO-3) in a mass ratio of 1:1.5:0.5.
[0092] Performance Testing
[0093] The biocoals of Examples 1 to 2 and Comparative Examples 1 to 7 were subjected to performance tests.
[0094] The thermal value and activation energy were determined according to GB / T 213-2008.
[0095] Refer to GB / T 9143-2021 to determine the drop strength and thermal stability.
[0096] The ash content of biocoal is determined with reference to GB / T 212-2008.
[0097] The test results are shown in Table 1.
[0098] Table 1 Performance test results
[0099]
[0100]
[0101] The results show that the biocoal prepared in Examples 1 to 2 has high calorific value, strong combustion performance, enhanced transportation and storage stability, improved safety during transportation, and low ash content. The biocoal in Examples 1 to 2 of the present invention has broad market value.
[0102] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A bio-coal, characterized in that: The invention comprises the following raw materials in parts by weight: 16 to 20 parts of bio-coal crystals, 10 to 14 parts of domestic sludge, 3 to 7 parts of corn cobs, 18 to 22 parts of modified agricultural waste, 0.4 to 0.8 parts of surfactant, 20 to 24 parts of binder and 120 to 130 parts of water; The preparation method of the bio-coal crystals is as follows: the cotton stalks are crushed into 1-2 cm, placed in a closed sintering furnace, heated to 500-700° C. under negative atmospheric pressure, kept warm for 6-9 hours, the sintering furnace stops heating and maintains negative pressure, cooled and crystallized to obtain bio-coal crystals; The preparation method of the modified agricultural waste is: (1) Crush cotton straw, peanut skin and corn straw respectively and select particles with a particle size of 60 to 100 meshes, mix the cotton straw, peanut skin and corn straw particles in a weight ratio of 2 to 3:1:0.3 to 0.8 to obtain mixed agricultural waste; (2) immersing the mixed agricultural waste in a sodium hydroxide aqueous solution having a mass fraction of 10 to 12%, heating the mixture to 80 to 90° C., and steaming the mixture for 140 to 160 minutes; filtering the mixture, and washing the mixture with water until the mixture is neutral, thereby obtaining alkalized agricultural waste; (3) adding water to the alkalized agricultural waste to make its moisture content 62-65wt%, adding a decomposing bacteria agent, and performing aerobic ventilated composting at a composting height of 1.3-1.6m. When the temperature of the pile body rises to 60-65°C, it is maintained for 8-10 days and the pile is turned; when the temperature rises to 50-55°C, it is maintained for 6-8 days, and the composting is completed; drying is performed to obtain modified agricultural waste with a moisture content of 40-45%; The decomposition agent is a compound of amylase, brewer's yeast and protease in a weight ratio of 1.3-1.5:1:0.4-0.7; The preparation method of the binder comprises the following steps: (1) Mix 1 part by weight of starch and 3 to 5 parts by weight of water, raise the temperature to 36° C. to 37° C., add 0.05 to 0.07 parts by weight of sodium chloride and 0.2 to 0.3 parts by weight of sodium hypochlorite, react for 6 to 8 hours, adjust the pH to 11.2 to 11.5, then add 0.1 to 0.15 parts by weight of sodium chloride and 0.2 to 0.25 parts by weight of propylene oxide in sequence, react at 36° C. to 37° C. for 25 to 30 hours, adjust the pH to neutral, and filter to obtain modified starch; (2) mixing diatomaceous earth, emulsified asphalt and modified starch in a weight ratio of 0.5 to 0.8:1:1.2 to 1.5 and stirring the mixture to obtain a binder; The surfactant is in a weight ratio of 1: 1.5~1.7:0.2~0.5 of sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium chloride and fatty alcohol polyoxyethylene ether.
2. The biocoal according to claim 1, characterized in that: The amount of the decomposing bacteria agent added is 0.2-0.4% of the weight of the alkalized agricultural waste.
3. The biocoal according to claim 1, characterized in that: The specific surface area of the diatomaceous earth is 20m 2 / g~30m 2 / g, and the pore radius is 100nm-200nm.
4. The biocoal according to claim 1, characterized in that: The emulsified asphalt is BLACKTROL produced by Shak Petroleum Technology Service Co., Ltd. ® HP emulsified asphalt.
5. The biocoal according to claim 1, characterized in that: The water content of domestic sludge is less than 75%.
6. A bio-coal production process according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1: Add bio-coal crystals, domestic sludge, corn cobs, modified agricultural waste, surfactants, binders and water into a kneader, knead evenly, and ripen for 3 to 4 hours to obtain a mixed material; Step 2: Press the mixed material into a shape, first dry it at 50-55° C. for 150-170 min, then dry it at 110-115° C. for 80-100 min, and obtain biocoal after cooling.
7. Use of the biocoal according to any one of claims 1 to 5 in the energy industry.
Citation Information
Patent Citations
Environmentally-friendly charcoal
CN103305307A
Preparation method for plant fuel by taking water hyacinth as raw material
CN103667363A
Modified asphalt binder and preparation method thereof
CN104830079A
Preparation method of biological coal
CN114525149A
Processes and systems for using biomineral by-products as a fuel and for NOx removal at coal burning power plants
US6405664B1