A secondary battery and its preparation method, and electric equipment

By doping fluorine into the positive and negative electrode active materials of lithium-ion batteries to form a charge network, the problems of interfacial charge transfer and diffusion resistance in lithium-ion batteries under low-temperature conditions are solved, thereby improving the low-temperature discharge capacity and energy retention rate, and enhancing the low-temperature performance and safety of the battery.

CN118398766BActive Publication Date: 2024-11-05CHINA FAW CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410842284.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-05
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

Lithium-ion batteries exhibit significant interfacial charge transfer resistance and diffusion resistance at low temperatures, leading to a decrease in energy density, and existing improvement measures are not very effective.

Method used

Fluorine is doped into the positive and negative electrode active materials to form a charge network, thereby reducing interfacial charge transfer and solid-phase diffusion resistance, while improving electrolyte wettability. The doping ratio and amount of fluorine are controlled to match the lithium-ion insertion and extraction capabilities.

Benefits of technology

It significantly improves the low-temperature discharge capacity and energy retention of lithium-ion batteries, enhances low-temperature performance, and improves battery safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present application provides a secondary battery and its preparation method and electrical equipment, belonging to the technical field of lithium-ion batteries. The secondary battery includes a positive electrode sheet and a negative electrode sheet, the positive electrode sheet includes a positive electrode active material, the negative electrode sheet includes a negative electrode active material, and the positive electrode active material and the negative electrode active material are doped with fluorine elements, which helps to improve the charge distribution on the surface and inside of the active material, form a strong electronegativity around the fluorine element, and have a strong electropositivity away from the fluorine element, thereby forming a charge network inside and on the surface of the active material. At low temperatures, this charge network can reduce the interfacial charge transfer impedance and solid-phase diffusion impedance of lithium ions and their electrons on the surface and inside of the active material, thereby improving the low-temperature discharge capacity and discharge energy. At the same time, the fluorine element has a good affinity with lithium ions, which helps to improve the wettability of the electrolyte to the active material, improve the lithium ion transmission effect, and improve the low-temperature performance of the lithium-ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a secondary battery and a preparation method thereof, and electrical equipment. Background Art

[0002] With the introduction of the "dual carbon" policy, new energy technologies have received more and more attention, such as wind energy, solar energy, tidal energy, hydrogen energy, etc. Compared with traditional energy, new energy is unstable, so it is generally used to store electrical energy through supporting energy storage batteries to achieve a stable supply of energy. The most widely used energy storage battery is lithium-ion battery, which has the advantages of high energy density, long cycle life, good fast charging performance, and good low temperature performance. On the other hand, with the popularization of new energy vehicles, lithium-ion secondary batteries for power batteries also have a wide range of application scenarios.

[0003] The optimal temperature for lithium-ion secondary batteries is about 25~35℃. When the temperature is below zero or even lower, below -20℃, the battery life is greatly reduced. At low temperatures, the interfacial charge transfer impedance and diffusion impedance of lithium-ion batteries increase significantly, and the polarization of the battery also increases significantly, so it is easier to reach the cut-off voltage, resulting in a decrease in energy density. At present, the low-temperature performance of lithium-ion batteries can generally be improved by coating or reducing the particle size at the material level, improving the formula or reducing the surface density at the pole level, and increasing the temperature rise or increasing the battery temperature at the cell level, but the improvement effect is still not obvious. How to significantly improve the low-temperature capability of lithium-ion batteries has become one of the current research focuses. Summary of the invention

[0004] The present application provides a secondary battery and a preparation method thereof, and an electrical device, which can improve the low-temperature performance of a lithium-ion battery.

[0005] The embodiment of the present application is implemented as follows:

[0006] In a first aspect, the present application example provides a secondary battery, which includes a positive electrode plate and a negative electrode plate, the positive electrode plate includes a positive electrode active material, the negative electrode plate includes a negative electrode active material, and both the positive electrode active material and the negative electrode active material are doped with fluorine element.

[0007] In the above technical solution, fluorine is a strong electron-withdrawing element. Both the positive electrode active material and the negative electrode active material are doped with fluorine, which helps to improve the charge distribution on the surface and inside of the active material, forming a strong electronegativity around the fluorine element and a strong electropositivity away from the fluorine element, thereby forming a charge network inside and on the surface of the active material. At low temperatures, this charge network can reduce the interfacial charge transfer impedance and solid-phase diffusion impedance of lithium ions and their electrons on the surface and inside of the active material, thereby improving the low-temperature discharge capacity and discharge energy. At the same time, fluorine has a good affinity with lithium ions, which helps to improve the wettability of the electrolyte to the active material, enhance the lithium ion transmission effect, and improve the low-temperature performance of lithium-ion batteries.

[0008] In some embodiments, the above R1 is the fluorine capacity ratio of the positive electrode active material, R2 is the fluorine capacity ratio of the negative electrode active material, and R1 and R2 satisfy 0.1≤R1 / R2≤10. Wherein, R1=M1 / C1, R2=M2 / C2, M1 is the mass ratio of fluorine element in the positive electrode active material to the positive electrode active material, M2 is the mass ratio of fluorine element in the negative electrode active material to the negative electrode active material, C1 is the reversible gram capacity of the positive electrode active material, and the unit of C1 is Ah / g, and C2 is the reversible gram capacity of the negative electrode active material, and the unit of C2 is Ah / g.

[0009] In the above example, fluorine doping is mainly for improving the lithium embedding effect. By making the fluorine content ratio of the positive electrode active material and the fluorine content ratio of the negative electrode active material satisfy 0.1≤R1 / R2≤10, the positive and negative electrode lithium ion embedding and extraction capabilities can be matched to avoid local aggregation of lithium ions, thereby improving the low-temperature discharge capacity retention rate and energy retention rate of the secondary battery, improving the lithium deposition of the secondary battery, and improving the safety of the secondary battery.

[0010] In some embodiments, the above R1 is the fluorine content ratio of the positive electrode active material, and R1 satisfies 0.01 g / Ah≤R1≤0.5 g / Ah;

[0011] Wherein, R1=M1 / C1, M1 is the mass ratio of fluorine element in the positive electrode active material to the positive electrode active material, C1 is the reversible gram capacity of the positive electrode active material, and the unit of C1 is Ah / g.

[0012] In the above example, fluorine doping is mainly to improve the lithium insertion effect. By making the fluorine content ratio of the positive electrode active material satisfy 0.01g / Ah≤R1≤0.5g / Ah, the fluorine doping amount can match the lithium insertion amount (fluorine mass ratio / gram capacity), which can not only ensure the lithium insertion ability of the positive electrode active material, but also enable the fluorine element to form a charge network inside and on the surface of the positive electrode active material, thereby effectively improving the interfacial charge transfer impedance and solid phase diffusion impedance on the surface and inside of the positive electrode active material, and improving the wettability of the electrolyte to the positive electrode active material, thereby improving the low temperature performance of the lithium-ion battery.

[0013] In some embodiments, the above R2 is the fluorine capacity ratio of the negative electrode active material, and R2 satisfies 0.01 g / Ah≤R2≤0.5 g / Ah;

[0014] Among them, R2=M2 / C2, M2 is the mass ratio of fluorine element in the negative electrode active material to the negative electrode active material, C2 is the reversible gram capacity of the positive electrode active material, and the unit of C2 is Ah / g.

[0015] In the above example, fluorine doping is mainly to improve the lithium insertion effect. By making the fluorine content ratio of the negative electrode active material satisfy 0.01g / Ah≤R2≤0.5g / Ah, the fluorine doping amount can match the lithium insertion amount (fluorine mass ratio / gram capacity), which can not only ensure the lithium insertion ability of the negative electrode active material, but also enable the fluorine element to form a charge network inside and on the surface of the negative electrode active material, thereby effectively improving the interface charge transfer impedance and solid phase diffusion impedance on the surface and inside of the negative electrode active material, and improving the wettability of the electrolyte to the negative electrode active material, thereby improving the low temperature performance of the lithium-ion battery.

[0016] In some embodiments, C1 is the reversible gram capacity of the positive electrode active material, and C1 satisfies 0.1 Ah / g≤C1≤0.25 Ah / g.

[0017] In some embodiments, C2 is the reversible gram capacity of the negative electrode active material, and C2 satisfies 0.2Ah / g≤C2≤0.8Ah / g.

[0018] In some embodiments, M1 is the mass ratio of fluorine element in the positive electrode active material to the positive electrode active material, and M1 satisfies 0.1%≤M1≤10%.

[0019] In some embodiments, the above M2 is the mass ratio of fluorine element in the negative electrode active material to the negative electrode active material, and M2 satisfies 0.1%≤M2≤10%.

[0020] In some embodiments, the positive electrode active material includes any one or more of lithium iron phosphate, nickel cobalt manganese ternary material, nickel cobalt aluminum ternary material, nickel cobalt manganese aluminum quaternary material, lithium cobalt oxide, lithium manganese oxide, lithium iron manganese phosphate and lithium nickel manganese oxide.

[0021] In some embodiments, the negative electrode active material includes any one or more of artificial graphite, natural graphite, mesocarbon microbeads, hard carbon, soft carbon, silicon, silicon oxygen, and silicon carbon.

[0022] In a second aspect, the present application provides a method for preparing the secondary battery, which includes: preparing a positive electrode active material and a negative electrode active material respectively.

[0023] The positive electrode active material is prepared by the following method: mixing the positive electrode active material and the fluorine-containing precursor, and then sintering in an inert gas atmosphere at a temperature of 300° C. to 700° C. for 2 h to 10 h;

[0024] The negative electrode active material is prepared by the following method: the negative electrode active material and the fluorine-containing precursor are mixed, and then sintered in an inert gas atmosphere at a temperature of 300° C. to 700° C. for 2 h to 10 h.

[0025] In the above technical solution, the method for preparing a secondary battery of the present application is conducive to preparing a secondary battery with a stable structure and good low-temperature performance.

[0026] In some embodiments, the fluorine-containing precursor includes polytetrafluoroethylene.

[0027] In a third aspect, the present application example provides an electrical device, which includes the above-mentioned secondary battery, and the secondary battery is used to provide electrical energy.

[0028] Compared with the prior art, this application has at least the following beneficial effects:

[0029] Fluorine is a strong electron-withdrawing element. Fluorine is doped in both the positive and negative active materials, which helps to improve the charge distribution on the surface and inside the active materials, forming a strong electronegativity around the fluorine element and a strong electropositivity away from the fluorine element, thereby forming a charge network inside and on the surface of the active material. At low temperatures, this charge network can reduce the interfacial charge transfer impedance and solid-phase diffusion impedance of lithium ions and their electrons on the surface and inside the active material, thereby improving the low-temperature discharge capacity and discharge energy. At the same time, fluorine has a good affinity with lithium ions, which helps to improve the wettability of the electrolyte to the active material, enhance the lithium ion transmission effect, and improve the low-temperature performance of lithium-ion batteries. DETAILED DESCRIPTION

[0030] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0031] The following is a detailed description of a secondary battery and a method for preparing the same according to an embodiment of the present application:

[0032] An embodiment of the present application provides a secondary battery, which includes a positive electrode sheet and a negative electrode sheet.

[0033] The positive electrode sheet includes a positive electrode active material layer and a positive electrode current collector. The positive electrode active material layer is combined with at least one side of the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material.

[0034] The negative electrode sheet includes a negative electrode active material layer and a negative electrode current collector. The negative electrode active material layer is combined with at least one side of the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material.

[0035] Both the positive electrode active material and the negative electrode active material are doped with fluorine element.

[0036] Fluorine is a strong electron-withdrawing element. Fluorine is doped in both the positive and negative active materials, which helps to improve the charge distribution on the surface and inside the active materials, forming a strong electronegativity around the fluorine element and a strong electropositivity away from the fluorine element, thereby forming a charge network inside and on the surface of the active material. At low temperatures, this charge network can reduce the interfacial charge transfer impedance and solid-phase diffusion impedance of lithium ions and their electrons on the surface and inside the active material, thereby improving the low-temperature discharge capacity and discharge energy. At the same time, fluorine has a good affinity with lithium ions, which helps to improve the wettability of the electrolyte to the active material, enhance the lithium ion transmission effect, and improve the low-temperature performance of lithium-ion batteries.

[0037] In some embodiments, R1 is the fluorine content ratio of the positive electrode active material, R2 is the fluorine content ratio of the negative electrode active material, and R1 and R2 satisfy 0.1≤R1 / R2≤10.

[0038] Among them, R1=M1 / C1, R2=M2 / C2, M1 is the mass ratio of fluorine element in the positive electrode active material to the positive electrode active material, M2 is the mass ratio of fluorine element in the negative electrode active material to the negative electrode active material, C1 is the reversible gram capacity of the positive electrode active material, and the unit of C1 is Ah / g, C2 is the reversible gram capacity of the negative electrode active material, and the unit of C2 is Ah / g.

[0039] As an example, the value of R1 / R2 can be 0.1, 0.2, 0.5, 0.8, 1, 2, 5, 8 or 10.

[0040] Fluorine doping is mainly to improve the lithium insertion effect. The lithium ion insertion and extraction capabilities of the positive and negative electrodes are matched. If one is extracted too quickly and the other is embedded too slowly, or one is extracted too slowly and the other is embedded too quickly, lithium ions will be locally aggregated, causing adverse effects. For example, when lithium ions are aggregated at the positive electrode, the low-temperature discharge capacity retention rate and energy retention rate of the secondary battery will decrease; when lithium ions are aggregated at the negative electrode, the low-temperature charging performance of the secondary battery will decrease, and lithium precipitation may occur, resulting in safety issues.

[0041] When the fluorine capacity ratio of the positive electrode active material and the fluorine capacity ratio of the negative electrode active material satisfy 0.1≤R1 / R2≤10, the lithium ion embedding and extraction capabilities of the positive and negative electrodes can be matched, avoiding local aggregation of lithium ions, thereby improving the low-temperature discharge capacity retention rate and energy retention rate of the secondary battery, improving the lithium plating of the secondary battery, and improving the safety of the secondary battery.

[0042] In some embodiments, R1 satisfies 0.01 g / Ah≤R1≤0.5 g / Ah.

[0043] As an example, the value of R1 may be 0.01 g / Ah, 0.1 g / Ah, 0.2 g / Ah, 0.3 g / Ah, 0.4 g / Ah, or 0.5 g / Ah.

[0044] Fluorine doping is mainly to improve the lithium insertion effect, that is, the fluorine doping amount needs to match the lithium insertion amount (fluorine mass ratio / gram capacity). When the fluorine capacity is relatively large, the fluorine doping amount is too high, or the lithium insertion ability of the active material is relatively low, the fluorine content is relatively large compared to the lithium ion content, and the excess fluorine will restrict the release of lithium ions, resulting in a decrease in the low-temperature performance of the secondary battery; when the fluorine capacity is relatively small, the fluorine doping amount is relatively small, or the lithium insertion ability of the active material is relatively high, the fluorine content is relatively small compared to the lithium ion content, and a strong and uniform charge network cannot be formed inside and on the surface of the active material, and the interfacial charge transfer impedance and solid-phase diffusion impedance on the surface and inside of the active material cannot be effectively improved, and the wettability of the electrolyte to the active material cannot be improved, and the low-temperature effect of the secondary battery is not obvious.

[0045] In the present application, by making the fluorine content ratio of the positive electrode active material satisfy 0.01g / Ah≤R1≤0.5g / Ah, the fluorine doping amount can match the lithium insertion amount (fluorine mass ratio / gram capacity), which can not only ensure the lithium insertion ability of the positive electrode active material, but also enable the fluorine element to form a charge network inside and on the surface of the positive electrode active material, thereby effectively improving the interface charge transfer impedance and solid phase diffusion impedance on the surface and inside of the positive electrode active material, and improving the wettability of the electrolyte to the positive electrode active material, thereby improving the low temperature performance of the lithium ion battery.

[0046] In some embodiments, R2 satisfies 0.01 g / Ah≤R2≤0.5 g / Ah.

[0047] As an example, the value of R2 may be 0.01 g / Ah, 0.1 g / Ah, 0.2 g / Ah, 0.3 g / Ah, 0.4 g / Ah, or 0.5 g / Ah.

[0048] In the present application, by making the fluorine content ratio of the negative electrode active material satisfy 0.01g / Ah≤R2≤0.5g / Ah, the fluorine doping amount can match the lithium insertion amount (fluorine mass ratio / gram capacity), which can not only ensure the lithium insertion ability of the negative electrode active material, but also enable the fluorine element to form a charge network inside and on the surface of the negative electrode active material, thereby effectively improving the interface charge transfer impedance and solid phase diffusion impedance on the surface and inside of the negative electrode active material, and improving the wettability of the electrolyte to the negative electrode active material, thereby improving the low temperature performance of the lithium ion battery.

[0049] In some embodiments, C1 satisfies 0.1 Ah / g≤C1≤0.25 Ah / g.

[0050] As an example, the value of C1 may be 0.1 Ah / g, 0.12 Ah / g, 0.15 Ah / g, 0.18 Ah / g, 0.2 Ah / g, 0.22 Ah / g, or 0.25 Ah / g.

[0051] In some embodiments, C2 satisfies 0.2Ah / g≤C2≤0.8Ah / g.

[0052] As an example, the value of C2 may be 0.2 Ah / g, 0.3 Ah / g, 0.4 Ah / g, 0.5 Ah / g, 0.6 Ah / g, 0.7 Ah / g, or 0.8 Ah / g.

[0053] In some embodiments, M1 satisfies 0.1%≤M1≤10%.

[0054] As examples, the value of M1 may be 0.1%, 0.2%, 0.5%, 1%, 2%, 5%, or 10%.

[0055] In some embodiments, M2 satisfies 0.1%≤M2≤10%.

[0056] As examples, the value of M2 may be 0.1%, 0.2%, 0.5%, 1%, 2%, 5%, or 10%.

[0057] In some embodiments, the positive electrode active material includes any one or more of lithium iron phosphate, nickel cobalt manganese ternary material, nickel cobalt aluminum ternary material, nickel cobalt manganese aluminum quaternary material, lithium cobalt oxide, lithium manganese oxide, lithium iron manganese phosphate and lithium nickel manganese oxide.

[0058] In some embodiments, the negative electrode active material includes any one or more of artificial graphite, natural graphite, mesocarbon microbeads, hard carbon, soft carbon, silicon, silicon oxygen, and silicon carbon.

[0059] The present application also provides a method for preparing a secondary battery, which comprises the following steps:

[0060] S1. Preparation of positive electrode sheet

[0061] S11. Preparation of positive electrode active material

[0062] The positive electrode active material and the fluorine-containing precursor are mixed according to a ratio, and then sintered in an inert gas atmosphere at a temperature of 300° C. to 700° C. for 2 h to 10 h to obtain a fluorine-doped positive electrode active material.

[0063] In some embodiments, the method of mixing the positive electrode active material and the fluorine-containing precursor comprises mechanical ball milling, and the time of the mechanical ball milling is 1 hour to 5 hours.

[0064] In some embodiments, the fluorine-containing precursor includes polytetrafluoroethylene.

[0065] The inert gas includes any one or more of nitrogen, helium, neon and xenon.

[0066] As an example, the sintering temperature may be 300° C., 350° C., 400° C., 450° C., 500° C., 550° C., 600° C., 650° C., or 700° C. The sintering time may be 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, or 10 h.

[0067] S12, prepare positive electrode sheet

[0068] The prepared fluorine-doped positive electrode active material, conductive carbon black (Super P), carbon nanotubes (CNT) and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 97:1:1:1, and solvent N-methylpyrrolidone (NMP) is added, and the mixture is fully stirred to obtain a positive electrode slurry; the prepared positive electrode slurry is evenly coated on a 16μm aluminum foil current collector, and a positive electrode sheet is prepared through processes such as drying, rolling, and cutting.

[0069] S2. Preparation of negative electrode sheet

[0070] S21. Preparation of negative electrode active material

[0071] The negative electrode active material and the fluorine-containing precursor are mixed according to a ratio, and then sintered in an inert gas atmosphere at a temperature of 300° C. to 700° C. for 2 h to 10 h to obtain a fluorine-doped negative electrode active material.

[0072] In some embodiments, the method of mixing the negative electrode active material and the fluorine-containing precursor comprises mechanical ball milling, and the time of the mechanical ball milling is 1 hour to 5 hours.

[0073] In some embodiments, the fluorine-containing precursor includes polytetrafluoroethylene.

[0074] The inert gas includes any one or more of nitrogen, helium, neon and xenon.

[0075] As an example, the sintering temperature may be 300° C., 350° C., 400° C., 450° C., 500° C., 550° C., 600° C., 650° C., or 700° C. The sintering time may be 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h, or 10 h.

[0076] S22. Preparation of negative electrode sheet

[0077] The prepared fluorine-doped negative electrode active material, carbon black (Super P), thickener sodium carboxymethyl cellulose (CMC), and binder styrene-butadiene rubber (SBR) are mixed in a mass ratio of 96:1:1:2, and deionized water is added and mixed evenly to obtain a negative electrode slurry; the prepared negative electrode slurry is evenly coated on a 10μm copper current collector, and a negative electrode sheet is prepared through processes such as drying, rolling, and cutting.

[0078] S3. Preparation of electrolyte

[0079] Ethylene carbonate, ethyl methyl carbonate, diethyl carbonate and propylene carbonate are uniformly mixed in a volume ratio of 1:1:1:1, and then dry high-purity LiPF6 is dissolved in the above mixed solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0080] S4. Preparation of isolation film

[0081] The selected diaphragm is a 9 μm polyethylene diaphragm coated on both sides with a ceramic coating with a thickness of 2 μm.

[0082] S5. Assembly

[0083] The prepared positive electrode sheet, separator, negative electrode sheet and electrolyte are assembled in sequence, so that the positive electrode sheet, separator, negative electrode sheet and separator are combined alternately, and a soft-pack battery with a capacity of 1Ah is obtained through formation.

[0084] A secondary battery and a preparation method thereof of the present application are further described in detail below in conjunction with embodiments.

[0085] Example 1

[0086] The present invention provides a secondary battery and a method for preparing the same, which comprises the following steps:

[0087] S1. Preparation of positive electrode sheet

[0088] S11. Preparation of positive electrode active material

[0089] The nickel-cobalt-manganese ternary material and polytetrafluoroethylene were mixed in a mass ratio of 10:1 and mechanically ball-milled for 2 hours, and then sintered in a nitrogen atmosphere at a temperature of 500°C for 5 hours to obtain a fluorine-doped positive electrode active material. The mass ratio M1 of the fluorine element in the positive electrode active material is 1.20%, the reversible gram capacity C1 of the positive electrode active material is 0.184Ah / g, and the fluorine capacity ratio R1 of the positive electrode active material is 0.065g / Ah.

[0090] S12, prepare positive electrode sheet

[0091] The prepared fluorine-doped positive electrode active material, conductive carbon black (Super P), carbon nanotubes (CNT) and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 97:1:1:1, and solvent N-methylpyrrolidone (NMP) is added, and the mixture is fully stirred to obtain a positive electrode slurry; the prepared positive electrode slurry is evenly coated on a 16μm aluminum foil current collector, and a positive electrode sheet is prepared through processes such as drying, rolling, and cutting.

[0092] S2. Preparation of negative electrode sheet

[0093] S21. Preparation of negative electrode active material

[0094] Artificial graphite and polytetrafluoroethylene were mixed in a mass ratio of 10:1 and mechanically ball-milled for 2 hours, and then sintered in a nitrogen atmosphere at a temperature of 500°C for 5 hours to obtain a fluorine-doped negative electrode active material. The mass ratio M2 of fluorine in the negative electrode active material is 2.57%, the reversible gram capacity C2 of the negative electrode active material is 0.346Ah / g, and the fluorine capacity ratio R2 of the negative electrode active material is 0.074g / Ah.

[0095] S22. Preparation of negative electrode sheet

[0096] The prepared fluorine-doped negative electrode active material, carbon black (Super P), thickener sodium carboxymethyl cellulose (CMC), and binder styrene-butadiene rubber (SBR) are mixed in a mass ratio of 96:1:1:2, and deionized water is added and mixed evenly to obtain a negative electrode slurry; the prepared negative electrode slurry is evenly coated on a 10μm copper current collector, and a negative electrode sheet is prepared through processes such as drying, rolling, and cutting.

[0097] S3. Preparation of electrolyte

[0098] Ethylene carbonate, ethyl methyl carbonate, diethyl carbonate and propylene carbonate are uniformly mixed in a volume ratio of 1:1:1:1, and then dry high-purity LiPF6 is dissolved in the above mixed solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0099] S4. Preparation of isolation film

[0100] The selected diaphragm is a 9 μm polyethylene diaphragm coated on both sides with a ceramic coating with a thickness of 2 μm.

[0101] S5. Assembly

[0102] The prepared positive electrode sheet, separator, negative electrode sheet and electrolyte are assembled in sequence, so that the positive electrode sheet, separator, negative electrode sheet and separator are combined alternately, and a soft-pack battery with a capacity of 1Ah is obtained through formation.

[0103] The ratio of the fluorine capacity ratio R1 of the positive electrode active material to the fluorine capacity ratio R2 of the negative electrode active material of the soft-pack battery in Example 1 of the present application is 0.878.

[0104] Comparative Example 1

[0105] The comparative example of the present application provides a secondary battery and a preparation method thereof, which comprises the following steps:

[0106] S1. Preparation of positive electrode sheet

[0107] The nickel-cobalt-manganese ternary material, conductive carbon black (Super P), carbon nanotubes (CNT) and binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 97:1:1:1, and the solvent N-methylpyrrolidone (NMP) was added and stirred to obtain a positive electrode slurry; the prepared positive electrode slurry was evenly coated on a 16μm aluminum foil current collector, and the positive electrode sheet was prepared through drying, rolling, cutting and other processes. The reversible gram capacity C1 of the positive active material is 0.193Ah / g.

[0108] S2. Preparation of negative electrode sheet

[0109] S21. Preparation of negative electrode active material

[0110] Artificial graphite and polytetrafluoroethylene were mixed in a mass ratio of 10:1 and mechanically ball-milled for 2 hours, and then sintered in a nitrogen atmosphere at 500°C for 5 hours to obtain a fluorine-doped negative electrode active material. The mass ratio M2 of fluorine in the negative electrode active material was 2.57%, the reversible gram capacity C2 of the negative electrode active material was 0.346Ah / g, and the fluorine capacity ratio R2 of the negative electrode active material was 0.074g / Ah.

[0111] S22. Preparation of negative electrode sheet

[0112] The prepared fluorine-doped negative electrode active material, carbon black (Super P), thickener sodium carboxymethyl cellulose (CMC), and binder styrene-butadiene rubber (SBR) are mixed in a mass ratio of 96:1:1:2, and deionized water is added and mixed evenly to obtain a negative electrode slurry; the prepared negative electrode slurry is evenly coated on a 10μm copper current collector, and a negative electrode sheet is prepared through processes such as drying, rolling, and cutting.

[0113] S3. Preparation of electrolyte

[0114] Ethylene carbonate, ethyl methyl carbonate, diethyl carbonate and propylene carbonate are uniformly mixed in a volume ratio of 1:1:1:1, and then dry high-purity LiPF6 is dissolved in the above mixed solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0115] S4. Preparation of isolation film

[0116] The selected diaphragm is a 9 μm polyethylene diaphragm coated on both sides with a ceramic coating with a thickness of 2 μm.

[0117] S5. Assembly

[0118] The prepared positive electrode sheet, separator, negative electrode sheet and electrolyte are assembled in sequence, so that the positive electrode sheet, separator, negative electrode sheet and separator are combined alternately, and a soft-pack battery with a capacity of 1Ah is obtained through formation.

[0119] Comparative Example 2

[0120] The comparative example of the present application provides a secondary battery and a preparation method thereof, which comprises the following steps:

[0121] S1. Preparation of positive electrode sheet

[0122] S11. Preparation of positive electrode active material

[0123] The nickel-cobalt-manganese ternary material and polytetrafluoroethylene were mixed in a mass ratio of 10:1 and mechanically ball-milled for 2 hours, and then sintered in a nitrogen atmosphere at a temperature of 500°C for 5 hours to obtain a fluorine-doped positive electrode active material. The mass ratio M1 of the fluorine element in the positive electrode active material is 1.20%, the reversible gram capacity C1 of the positive electrode active material is 0.184Ah / g, and the fluorine capacity ratio R1 of the positive electrode active material is 0.065g / Ah.

[0124] S12, prepare positive electrode sheet

[0125] The prepared fluorine-doped positive electrode active material, conductive carbon black (Super P), carbon nanotubes (CNT) and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 97:1:1:1, and solvent N-methylpyrrolidone (NMP) is added, and the mixture is fully stirred to obtain a positive electrode slurry; the prepared positive electrode slurry is evenly coated on a 16μm aluminum foil current collector, and a positive electrode sheet is prepared through processes such as drying, rolling, and cutting.

[0126] S2. Preparation of negative electrode sheet

[0127] Artificial graphite, carbon black (Super P), thickener sodium carboxymethyl cellulose (CMC), binder styrene butadiene rubber (SBR) were mixed in a mass ratio of 96:1:1:2, deionized water was added, and the mixture was uniformly mixed to obtain negative electrode slurry; the obtained negative electrode slurry was uniformly coated on a 10μm copper current collector, and the negative electrode sheet was prepared through drying, rolling, cutting and other processes. The reversible gram capacity C2 of the negative electrode active material is 0.365Ah / g.

[0128] S3. Preparation of electrolyte

[0129] Ethylene carbonate, ethyl methyl carbonate, diethyl carbonate and propylene carbonate are uniformly mixed in a volume ratio of 1:1:1:1, and then dry high-purity LiPF6 is dissolved in the above mixed solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0130] S4. Preparation of isolation film

[0131] The selected diaphragm is a 9 μm polyethylene diaphragm coated on both sides with a ceramic coating with a thickness of 2 μm.

[0132] S5. Assembly

[0133] The prepared positive electrode sheet, separator, negative electrode sheet and electrolyte are assembled in sequence, so that the positive electrode sheet, separator, negative electrode sheet and separator are combined alternately, and a soft-pack battery with a capacity of 1Ah is obtained through formation.

[0134] Comparative Example 3

[0135] The comparative example of the present application provides a secondary battery and a preparation method thereof, which comprises the following steps:

[0136] S1. Preparation of positive electrode sheet

[0137] The nickel-cobalt-manganese ternary material, conductive carbon black (Super P), carbon nanotubes (CNT) and binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 97:1:1:1, and the solvent N-methylpyrrolidone (NMP) was added and stirred to obtain a positive electrode slurry; the prepared positive electrode slurry was evenly coated on a 16μm aluminum foil current collector, and the positive electrode sheet was prepared through drying, rolling, cutting and other processes. The reversible gram capacity C1 of the positive active material is 0.193Ah / g.

[0138] S2. Preparation of negative electrode sheet

[0139] Artificial graphite, carbon black (Super P), thickener sodium carboxymethyl cellulose (CMC), binder styrene butadiene rubber (SBR) were mixed in a mass ratio of 96:1:1:2, deionized water was added, and the mixture was uniformly mixed to obtain negative electrode slurry; the obtained negative electrode slurry was uniformly coated on a 10μm copper current collector, and the negative electrode sheet was prepared through drying, rolling, cutting and other processes. The reversible gram capacity C2 of the negative electrode active material is 0.365Ah / g.

[0140] S3. Preparation of electrolyte

[0141] Ethylene carbonate, ethyl methyl carbonate, diethyl carbonate and propylene carbonate are uniformly mixed in a volume ratio of 1:1:1:1, and then dry high-purity LiPF6 is dissolved in the above mixed solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0142] S4. Preparation of isolation film

[0143] The selected diaphragm is a 9 μm polyethylene diaphragm coated on both sides with a ceramic coating with a thickness of 2 μm.

[0144] S5. Assembly

[0145] The prepared positive electrode sheet, separator, negative electrode sheet and electrolyte are assembled in sequence, so that the positive electrode sheet, separator, negative electrode sheet and separator are combined alternately, and a soft-pack battery with a capacity of 1Ah is obtained through formation.

[0146] Examples 2 to 16 Secondary batteries were prepared according to the method of Example 1, and relevant parameters of the secondary batteries of Examples 1 to 16 and Comparative Examples 1 to 3 are shown in Table 1.

[0147] Table 1 Relevant parameters of the secondary batteries of Examples 1 to 16 and Comparative Examples 1 to 3

[0148]

[0149] Among them, M1, M2, C1 and C2 are measured by the following method:

[0150] According to GB / T 21057-2007 "General method for determination of fluorine content in inorganic chemical products - ion selective electrode method", the fluorine content of positive electrode active materials and negative electrode active materials is determined and converted into mass percentage, namely M1 and M2.

[0151] According to the above method for preparing soft-pack electrode sheets, prepare single-sided button sheets, assemble the single-sided button sheets with diaphragms, lithium sheets and gaskets or springs into button batteries, and the electrolyte is consistent with the soft-pack electrolyte. The button battery is charged and discharged for 3 cycles at a rate of 0.1C. The charge and discharge cut-off voltage is differentiated according to the different materials. The cut-off voltage of different materials is recognized by professionals in this field. The ratio of the delithiation capacity of the last cycle to the mass of the active material is the reversible gram capacity C1 of the positive active material and the reversible gram capacity C2 of the negative active material.

[0152] Test Example 1

[0153] The low temperature capacity retention rate and low temperature energy retention rate of the secondary batteries prepared in Examples 1 to 16 and Comparative Examples 1 to 3 were measured respectively. The results are shown in Table 2.

[0154] The test method is as follows:

[0155] (1) Low temperature capacity retention rate

[0156] At 25°C, charge the battery to the upper cut-off voltage at a constant current and voltage rate of 0.33C (the constant voltage cut-off current is 0.05C), and then discharge it to the lower cut-off voltage at a constant current rate of 0.33C. Cycle 3 cycles under this charge and discharge condition, and record the discharge capacity of the last cycle as the 25°C discharge capacity. Continue to charge the battery to the upper cut-off voltage at a constant current and voltage rate of 0.33C at 25°C (the constant voltage cut-off current is 0.05C), then place the battery at -20°C for 3 hours, and then discharge it to the lower cut-off voltage at a constant current rate of 0.33C, and record the discharge capacity as the -20°C discharge capacity. The ratio of the -20°C discharge capacity to the 25°C discharge capacity is recorded as the low temperature capacity retention rate.

[0157] (2) Low temperature energy retention rate

[0158] At 25℃, charge the battery to the upper cut-off voltage at a constant current and voltage rate of 0.33C (the constant voltage cut-off current is 0.05C), and then discharge it to the lower cut-off voltage at a constant current rate of 0.33C. Cycle 3 cycles under this charge and discharge condition, and record the discharge energy of the last cycle as the 25℃ discharge energy. Continue to charge the battery to the upper cut-off voltage at a constant current and voltage rate of 0.33C at 25℃ (the constant voltage cut-off current is 0.05C), then place the battery at -20℃ for 3h, and then discharge it to the lower cut-off voltage at a constant current rate of 0.33C. Record the discharge capacity as the -20℃ discharge energy. The ratio of the -20℃ discharge energy to the 25℃ discharge energy is recorded as the low-temperature energy retention rate.

[0159] Table 2 Low temperature capacity retention rate and low temperature energy retention rate of the secondary batteries prepared in Examples 1 to 16 and Comparative Examples 1 to 3

[0160]

[0161] It can be seen from Examples 1 to 2 that when the mass ratio M1 of the fluorine element in the positive electrode active material to the positive electrode active material satisfies 0.1%≤M1≤10%, and the mass ratio M2 of the fluorine element in the negative electrode active material to the negative electrode active material satisfies 0.1%≤M2≤10%, the reversible gram capacity C1 of the positive electrode active material satisfies 0.1Ah / g≤C1≤0.25Ah / g, and the reversible gram capacity C2 of the negative electrode active material satisfies 0.2Ah / g≤C2≤0.8Ah / g , the fluorine content ratio R1 of the positive electrode active material satisfies 0.01g / Ah≤R1≤0.5g / Ah, the fluorine content ratio R2 of the negative electrode active material satisfies 0.01g / Ah≤R2≤0.5g / Ah, and when the ratio of the fluorine content ratio R1 of the positive electrode active material and the fluorine content ratio R2 of the negative electrode active material of the secondary battery satisfies 0.1≤R1 / R2≤10, the low-temperature capacity retention rate of the secondary battery is above 87.1%, and the low-temperature energy retention rate is above 83.3%.

[0162] By comparing Examples 3 to 4 with Examples 1 to 2, it can be seen that when the ratio of the fluorine capacity ratio R1 of the positive electrode active material and the fluorine capacity ratio R2 of the negative electrode active material of the secondary battery does not satisfy 0.1≤R1 / R2≤10, but the mass ratio M1 of the fluorine element in the positive electrode active material satisfies 0.1%≤M1≤10%, the mass ratio M2 of the fluorine element in the negative electrode active material satisfies 0.1%≤M2≤10%, the reversible gram capacity C1 of the positive electrode active material satisfies 0.1Ah / g≤C1≤0.25Ah / g, and the reversible gram capacity C2 of the negative electrode active material satisfies 0.2Ah / g≤C2≤0.8Ah / g, the low-temperature capacity retention rate of the secondary battery is lower than that of Examples 1 to 2, and the low-temperature energy retention rate is lower than that of Examples 1 to 2.

[0163] By comparing Examples 5 to 6 with Examples 1 to 2, it can be seen that when the fluorine content ratio R1 of the positive electrode active material does not satisfy 0.01g / Ah≤R1≤0.5g / Ah, but the mass ratio M1 of the fluorine element in the positive electrode active material satisfies 0.1%≤M1≤10%, the mass ratio M2 of the fluorine element in the negative electrode active material satisfies 0.1%≤M2≤10%, the reversible gram capacity C1 of the positive electrode active material satisfies 0.1Ah / g≤C1≤0.25Ah / g, the reversible gram capacity C2 of the negative electrode active material satisfies 0.2Ah / g≤C2≤0.8Ah / g, and the fluorine content ratio R2 of the negative electrode active material satisfies 0.01g / Ah≤R2≤0.5g / Ah, the low-temperature capacity retention rate of the secondary battery is lower than that of Examples 1 to 2, and the low-temperature energy retention rate is lower than that of Examples 1 to 2.

[0164] By comparing Examples 7 to 8 with Examples 1 to 2, it can be seen that when the fluorine content ratio R2 of the negative electrode active material does not satisfy 0.01g / Ah≤R2≤0.5g / Ah, but the mass ratio M1 of the fluorine element in the positive electrode active material satisfies 0.1%≤M1≤10%, the mass ratio M2 of the fluorine element in the negative electrode active material satisfies 0.1%≤M2≤10%, the reversible gram capacity C1 of the positive electrode active material satisfies 0.1Ah / g≤C1≤0.25Ah / g, and the fluorine content ratio R1 of the positive electrode active material satisfies 0.01g / Ah≤R1≤0.5g / Ah, the low-temperature capacity retention rate of the secondary battery is lower than that of Examples 1 to 2, and the low-temperature energy retention rate is lower than that of Examples 1 to 2.

[0165] By comparing Examples 9 to 10 with Examples 1 to 8, it can be seen that when the mass ratio M1 of fluorine element in the positive electrode active material does not satisfy 0.1%≤M1≤10%, but the mass ratio M2 of fluorine element in the negative electrode active material satisfies 0.1%≤M2≤10%, the reversible gram capacity C1 of the positive electrode active material satisfies 0.1Ah / g≤C1≤0.25Ah / g, and the reversible gram capacity C2 of the negative electrode active material satisfies 0.2Ah / g≤C2≤0.8Ah / g, the low-temperature capacity retention rate of the secondary battery is lower than that of Examples 1 to 8, and the low-temperature energy retention rate is lower than that of Examples 1 to 8.

[0166] By comparing Examples 11 to 12 with Examples 1 to 8, it can be seen that when the mass ratio M2 of fluorine element in the negative electrode active material does not satisfy 0.1%≤M2≤10%, but the mass ratio M1 of fluorine element in the positive electrode active material satisfies 0.1%≤M1≤10%, the reversible gram capacity C1 of the positive electrode active material satisfies 0.1Ah / g≤C1≤0.25Ah / g, and the reversible gram capacity C2 of the negative electrode active material satisfies 0.2Ah / g≤C2≤0.8Ah / g, the low-temperature capacity retention rate of the secondary battery is lower than that of Examples 1 to 8, and the low-temperature energy retention rate is lower than that of Examples 1 to 8.

[0167] By comparing Examples 13 to 14 with Examples 1 to 8, it can be seen that when the reversible gram capacity C1 of the positive electrode active material does not satisfy 0.1Ah / g≤C1≤0.25Ah / g, but the mass ratio M1 of the fluorine element in the positive electrode active material satisfies 0.1%≤M1≤10%, the mass ratio M2 of the fluorine element in the negative electrode active material satisfies 0.1%≤M2≤10%, and the reversible gram capacity C2 of the negative electrode active material satisfies 0.2Ah / g≤C2≤0.8Ah / g, the low-temperature capacity retention rate of the secondary battery is lower than that of Examples 1 to 8, and the low-temperature energy retention rate is lower than that of Examples 1 to 8.

[0168] By comparing Examples 15 to 16 with Examples 1 to 8, it can be seen that when the reversible gram capacity C2 of the negative electrode active material does not satisfy 0.2Ah / g≤C2≤0.8Ah / g, but the mass ratio M1 of the fluorine element in the positive electrode active material satisfies 0.1%≤M1≤10%, the mass ratio M2 of the fluorine element in the negative electrode active material satisfies 0.1%≤M2≤10%, and the reversible gram capacity C1 of the positive electrode active material satisfies 0.1Ah / g≤C1≤0.25Ah / g, the low-temperature capacity retention rate of the secondary battery is lower than that of Examples 1 to 8, and the low-temperature energy retention rate is lower than that of Examples 1 to 8.

[0169] By comparing Comparative Example 1 with Examples 1 to 16, it can be seen that the positive electrode active material of Comparative Example 1 is not doped with fluorine, and the low-temperature capacity retention rate of its secondary battery is only 72.3%, which is lower than that of Examples 1 to 16, and the low-temperature energy retention rate is only 68.5%, which is lower than that of Examples 1 to 14 and 16.

[0170] By comparing Comparative Example 2 with Examples 1 to 16, it can be seen that the negative electrode active material of Comparative Example 2 is not doped with fluorine, and the low-temperature capacity retention rate of its secondary battery is only 70.5%, which is lower than that of Examples 1 to 16, and the low-temperature energy retention rate is only 66.2%, which is lower than that of Examples 1 to 16.

[0171] By comparing Comparative Example 3 with Examples 1 to 16, it can be seen that neither the positive electrode active material nor the negative electrode active material of Comparative Example 3 is doped with fluorine element, and the low-temperature capacity retention rate of its secondary battery is only 65.6%, which is lower than that of Examples 1 to 16, and the low-temperature energy retention rate is only 60.4%, which is lower than that of Examples 1 to 16.

[0172] The above description is only a specific embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A secondary battery, characterized in that: The secondary battery comprises a positive electrode sheet and a negative electrode sheet, the positive electrode sheet comprises a positive electrode active material, the negative electrode sheet comprises a negative electrode active material, and both the positive electrode active material and the negative electrode active material are doped with fluorine element; R1 is the fluorine capacity ratio of the positive electrode active material, R2 is the fluorine capacity ratio of the negative electrode active material, and R1 and R2 satisfy 0.1≤R1 / R2≤10; Among them, R1=M1 / C1, R2=M2 / C2, M1 is the mass ratio of fluorine element in the positive electrode active material to the positive electrode active material, M2 is the mass ratio of fluorine element in the negative electrode active material to the negative electrode active material, C1 is the reversible gram capacity of the positive electrode active material, and the unit of C1 is Ah / g, C2 is the reversible gram capacity of the negative electrode active material, and the unit of C2 is Ah / g.

2. The secondary battery according to claim 1, characterized in that: R1 is the fluorine content ratio of the positive electrode active material, and R1 satisfies 0.01 g / Ah≤R1≤0.5 g / Ah; Wherein, R1=M1 / C1, M1 is the mass ratio of fluorine element in the positive electrode active material to the positive electrode active material, C1 is the reversible gram capacity of the positive electrode active material, and the unit of C1 is Ah / g.

3. The secondary battery according to claim 1, characterized in that: R2 is the fluorine capacity ratio of the negative electrode active material, and R2 satisfies 0.01 g / Ah≤R2≤0.5 g / Ah; Wherein, R2=M2 / C2, M2 is the mass ratio of fluorine element in the negative electrode active material to the negative electrode active material, C2 is the reversible gram capacity of the positive electrode active material, and the unit of C2 is Ah / g.

4. The secondary battery according to claim 1, characterized in that: C1 is the reversible gram capacity of the positive electrode active material, and C1 satisfies 0.1Ah / g≤C1≤0.25Ah / g.

5. The secondary battery according to claim 1, characterized in that: C2 is the reversible gram capacity of the negative electrode active material, and C2 satisfies 0.2Ah / g≤C2≤0.8Ah / g.

6. The secondary battery according to claim 1, characterized in that: M1 is the mass ratio of fluorine element in the positive electrode active material to the positive electrode active material, and M1 satisfies 0.1%≤M1≤10%.

7. The secondary battery according to claim 1, characterized in that: M2 is the mass ratio of fluorine element in the negative electrode active material to the negative electrode active material, and M2 satisfies 0.1%≤M2≤10%.

8. The secondary battery according to claim 1, characterized in that: The positive electrode active material includes any one or more of lithium iron phosphate, nickel-cobalt-manganese ternary material, nickel-cobalt-aluminum ternary material, nickel-cobalt-manganese-aluminum quaternary material, lithium cobalt oxide, lithium manganese oxide, lithium iron manganese phosphate and lithium nickel manganese oxide.

9. The secondary battery according to claim 1, characterized in that: The negative electrode active material includes any one or more of artificial graphite, natural graphite, mesophase carbon microbeads, hard carbon, soft carbon, silicon, silicon oxygen and silicon carbon.

10. An electrical device, characterized in that: The electrical equipment comprises the secondary battery according to any one of claims 1 to 9, and the secondary battery is used to provide electrical energy.