A kind of gypsum water reducing agent and preparation method thereof

By using a polycarboxylate water-reducing agent polymerized with EPEG and acrylic acid in gypsum, and combining modified cellulose and polyaniline grafted SiO2, the problems of poor applicability and low water-reducing rate of existing gypsum water-reducing agents have been solved, significantly improving It improves the fluidity and strength of gypsum and promotes the application of gypsum-based materials.

CN118405874BActive Publication Date: 2024-10-29张豹
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410521741.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-28
Publication Date
2024-10-29
Estimated Expiration
2044-04-28

AI Technical Summary

Technical Problem

Existing gypsum water-reducing agents have poor applicability, low water-reducing rate, and insignificant reinforcing effect, resulting in damage to the density and strength of gypsum-based materials, limiting their large-scale application.

Method used

A polycarboxylate water-reducing agent based on the polymerization of ethylene glycol monovinyl polyoxyethylene ether (EPEG) and acrylic acid is used, combined with modified cellulose and polyaniline grafted SiO2 to improve the fluidity of gypsum through hydrogen bonding and hydrophobicity. and intensity.

Benefits of technology

It significantly improves the water reduction rate and strength of gypsum, enhances applicability, and has significant application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004815324600000081
    Figure BDA0004815324600000081
Patent Text Reader

Abstract

The present invention belongs to the technical field of water reducing agents, and specifically relates to a gypsum water reducing agent and a preparation method thereof. The gypsum water reducing agent, by weight, comprises: 260-280 parts of EPEG, 20-30 parts of acrylic acid, 1-2 parts of mercaptoethanol, 10-15 parts of modified cellulose, 10-20 parts of polyaniline grafted SiO2, 0.5-1 part of ascorbic acid, 3-5 parts of hydrogen peroxide and 20-30 parts of NaOH solution, and 250-300 parts of water. The gypsum water reducing agent provided by the present invention can effectively improve the water reduction rate of the water reducing agent in gypsum materials, while improving the strength of gypsum, has good applicability, and has significant application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of water reducing agents, and particularly relates to a gypsum water reducing agent and a preparation method thereof. Background Art

[0002] Gypsum products have the characteristics of thermal insulation, sound absorption, and environmental protection, and are known as "green cement". However, the actual mixing water requirement of gypsum products is much greater than the theoretical water requirement, resulting in increased porosity and low density of gypsum products. Adding water reducer to gypsum can not only reduce the amount of water used to mix gypsum and increase the fluidity of gypsum, but also improve the time-dependent loss of gypsum fluidity. In addition, better gypsum water reducers have greater fluidity, and the initial setting time of gypsum will also increase, that is, they have a certain retarding effect.

[0003] At present, the gypsum water reducer used in practical applications is mostly polycarboxylic acid water reducer for concrete. When it is directly added to gypsum, there are generally problems such as poor applicability, low water reduction rate, unclear reinforcement effect, and damaged strength. These have greatly restricted the large-scale application and development of gypsum-based materials. Therefore, it is of great practical value to study a water reducer specifically suitable for gypsum. Summary of the invention

[0004] In view of the fact that most gypsum water-reducing agents used in the prior art are concrete water-reducing agents, which are directly added to semi-hydrated gypsum, generally have the problems of poor applicability, low water reduction rate, unclear reinforcement effect, damaged strength, etc., the present invention provides a gypsum water-reducing agent, which belongs to a polycarboxylic acid water-reducing agent, is based on the polymerization of ethylene glycol monovinyl polyoxyethylene ether (EPEG) and acrylic acid, uses modified cellulose and polyaniline grafted SiO2 as auxiliary phases, can effectively improve the water reduction rate of the water-reducing agent in gypsum materials, and at the same time improve the strength of gypsum, has good applicability, and has significant application prospects.

[0005] The first aspect of the present invention provides a gypsum water reducer, which comprises, by weight, 260 to 280 parts of EPEG, 20 to 30 parts of acrylic acid, 1 to 2 parts of mercaptoethanol, 10 to 15 parts of modified cellulose, 10 to 20 parts of polyaniline grafted SiO2, 0.5 to 1 part of ascorbic acid, 3 to 5 parts of hydrogen peroxide, 20 to 30 parts of NaOH solution, and 250 to 300 parts of water.

[0006] The preparation method of the modified cellulose comprises:

[0007] The cellulose is soaked in a phytic acid solution containing ammonium persulfate for 3 to 4 hours, then dicyanoammonium phosphate is added, and the cellulose is modified under hydrothermal conditions, washed, and dried to obtain modified cellulose.

[0008] Furthermore, the mass concentration of the phytic acid solution is 10-20%, the mass ratio of ammonium persulfate to phytic acid is 1:2-3; and the mass ratio of dicyanammonium phosphate to cellulose is 1-2:5-6.

[0009] Furthermore, after adding dicyanammonium phosphate, a hydrothermal reaction is carried out at 160° C. to 180° C. for 10 to 12 hours.

[0010] Furthermore, the preparation method of polyaniline grafted SiO2 comprises the following steps:

[0011] S1: dissolving tetraethyl orthosilicate in ethanol, adding ammonium bicarbonate after sufficient stirring, mixing well and placing in a hydrothermal reactor for hydrothermal reaction, filtering, washing and drying to prepare SiO2 material;

[0012] S2: Dispersing SiO2 material and hexamethylene diisocyanate in acetone, then adding dibutyltin dilaurate, fully reacting under heating conditions, and then filtering, washing, and drying to prepare isocyanate SiO2;

[0013] S3: Dissolve isocyanate-treated nano-SiO2 in ethanol, disperse it evenly by ultrasonication, then add aniline to react for 2-3 hours, then drop dilute hydrochloric acid, and then add ammonium persulfate to continue the reaction. After filtering, washing and drying, polyaniline-grafted SiO2 is prepared.

[0014] Furthermore, in step S1, the mass ratio of tetraethyl orthosilicate, ammonium bicarbonate and ethanol is 1.5-2:1:40-50; the temperature of the hydrothermal reaction is 160-180° C., and the time is 16-20 hours.

[0015] Furthermore, in step S2, the mass ratio of SiO2 material, hexamethylene diisocyanate, dibutyltin dilaurate, and acetone is 1:1.2-1.5:0.01-0.015:40-50.

[0016] Furthermore, after adding dibutyltin dilaurate, the mixture is heated to 80-90° C. and refluxed for 5-6 hours.

[0017] Furthermore, in step S2, the SiO2 material and hexamethylene diisocyanate are dispersed in acetone by ultrasonic dispersion in a nitrogen environment.

[0018] Furthermore, in step S3, the mass ratio of isocyanate-treated nano-SiO2, aniline, ammonium persulfate and ethanol is 1:1.5-2:6-8:40-50.

[0019] Furthermore, the concentration of the dilute hydrochloric acid is 1 mol / L, and the mass ratio of the dilute hydrochloric acid to the ethanol is 1:45-50.

[0020] Further, after adding ammonium persulfate, react for 6 to 8 hours and then filter.

[0021] Furthermore, the mass fraction of the NaOH solution is 20% to 30%; the mass fraction of the hydrogen peroxide is 30%.

[0022] The second aspect of the present invention provides a method for preparing the above-mentioned gypsum water reducing agent, comprising the following steps:

[0023] (1) Add EPEG, modified cellulose, polyaniline-grafted SiO2 and water into a round-bottom flask and stir thoroughly to dissolve to form a mixed solution A;

[0024] (2) mixing acrylic acid, mercaptoethanol and water, and stirring thoroughly to form a mixed solution B;

[0025] (3) mixing ascorbic acid and water, and stirring thoroughly to form a mixed solution C;

[0026] (4) Add hydrogen peroxide to mixed solution A, stir for 10 to 20 minutes, then simultaneously add mixed solution B and mixed solution C dropwise, and continue the reaction for 1 to 1.5 hours after the addition is complete;

[0027] (5) Adding NaOH solution to the mixed solution obtained in step (4) to control the pH value to 6-8, and then filtering, washing and drying to obtain a gypsum water reducing agent.

[0028] Furthermore, the dropwise addition time of the mixed solution B is 1 to 1.1 hours, and the dropwise addition time of the mixed solution C is 1.2 to 1.3 hours.

[0029] The beneficial effects achieved by one or more technical solutions of the present invention are as follows:

[0030] 1. The preparation of polyacid water reducers based on the polymerization reaction of EPEG and acrylic acid is a commonly used method in this field. However, the prepared water reducer is directly added to gypsum. Although it can change the interface structure and electrochemical properties of gypsum particles through adsorption and play a dispersing role through the double layer repulsion effect and steric hindrance effect, in fact, the hydration rate of gypsum is too fast, which will lead to the water reducer being unable to effectively improve the problem of excessive loss of gypsum-based fluidity.

[0031] The present invention simultaneously adds phytic acid, phosphorus-synergistically modified cellulose and polyaniline-grafted SiO2 into the system, mainly considering that the phytic acid molecular structure contains phosphorus oxygen groups, which are good hydrogen bond receptors and can form strong hydrogen bonds with the hydroxyl groups on the cellulose and the amino groups on the polyaniline. The presence of hydrogen bonds can form a tight structure between the components in the system, slowing down the hydration speed of the gypsum as a whole, and effectively improving the strength of the gypsum. Moreover, the modification of phosphorus on cellulose can improve the collapse-preserving performance of the water-reducing agent and improve the retarding effect. In addition, the polyaniline-grafted SiO2 material has a good hydrophobic effect and can further reduce the hydration rate.

[0032] 2. The gypsum water-reducing agent provided by the present invention can effectively improve the water-reducing rate of the water-reducing agent in the gypsum material, while improving the strength of the gypsum, has good applicability, and has significant application prospects. DETAILED DESCRIPTION

[0033] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in combination with specific embodiments and comparative examples.

[0034] Example 1

[0035] This embodiment provides a gypsum water reducing agent, which is composed of the following raw materials in parts by weight:

[0036] 260 parts of EPEG, 20 parts of acrylic acid, 1 part of mercaptoethanol, 10 parts of modified cellulose, 10 parts of polyaniline grafted SiO2, 0.5 parts of ascorbic acid, 3 parts of 30% hydrogen peroxide, 20 parts of 20% NaOH solution, 260 parts of water;

[0037] The preparation method of the gypsum water reducing agent is:

[0038] (1) Preparation of modified cellulose:

[0039] The cellulose was immersed in a phytic acid solution containing ammonium persulfate for 3 hours (the mass concentration of the phytic acid solution was 10%, and the mass ratio of ammonium persulfate to phytic acid was 1:2), and then dicyanoammonium phosphate was added (the mass ratio of dicyanoammonium phosphate to cellulose was 1:5), and the cellulose was modified by reacting under hydrothermal conditions at 160°C for 12 hours, and then washed and dried to obtain modified cellulose.

[0040] (2) Preparation of polyaniline grafted SiO2:

[0041] S1: dissolving tetraethyl orthosilicate in ethanol, adding ammonium bicarbonate (the mass ratio of tetraethyl orthosilicate, ammonium bicarbonate and ethanol is 1.5:1:40) after sufficient stirring, placing in a hydrothermal reactor after mixing, performing hydrothermal reaction at 180°C for 16h, filtering, washing and drying to prepare SiO2 material;

[0042] S2: Disperse SiO2 material and hexamethylene diisocyanate in acetone, perform ultrasonic dispersion in a nitrogen environment, then add dibutyltin dilaurate (the mass ratio of SiO2 material, hexamethylene diisocyanate, dibutyltin dilaurate, and acetone is 1:1.2:0.015:40), heat to 90°C for reflux reaction for 5 hours, and then filter, wash, and dry to prepare isocyanate SiO2;

[0043] S3: Dissolve isocyanate nano-SiO2 in ethanol, disperse it evenly with ultrasound, then add aniline to react for 3 hours, then add 1 mol / L dilute hydrochloric acid to create an acidic environment (the mass ratio of dilute hydrochloric acid to ethanol is 1:45), then add ammonium persulfate to continue reacting for 6 hours (the mass ratio of isocyanate nano-SiO2, aniline, ammonium persulfate, and ethanol is 1:1.5:6:50), filter, wash, and dry to prepare polyaniline-grafted SiO2.

[0044] (3) Add EPEG, modified cellulose, polyaniline-grafted SiO2 and 150 parts of water into a round-bottom flask and stir thoroughly to dissolve to form a mixed solution A;

[0045] (4) mixing acrylic acid, mercaptoethanol and 80 parts of water, and stirring thoroughly to form a mixed solution B;

[0046] (5) Mix ascorbic acid and 30 parts of water and stir thoroughly to form a mixed solution C;

[0047] (6) Add hydrogen peroxide to mixed solution A, stir for 10 min, and then simultaneously add mixed solution B and mixed solution C. The addition time of mixed solution B is 1 h, and the addition time of mixed solution C is 1.2 h. After the addition is completed, the reaction is continued for 1 h.

[0048] (7) Adding NaOH solution to the mixed solution obtained in step (6) to control the pH value to 6-8, and then filtering, washing and drying to obtain a gypsum water reducing agent.

[0049] Example 2

[0050] This embodiment provides a gypsum water reducing agent, which is composed of the following raw materials in parts by weight:

[0051] 270 parts of EPEG, 30 parts of acrylic acid, 2 parts of mercaptoethanol, 15 parts of modified cellulose, 15 parts of polyaniline grafted SiO2, 1 part of ascorbic acid, 5 parts of 30% hydrogen peroxide, 25 parts of 20% NaOH solution, and 280 parts of water;

[0052] The preparation method of the gypsum water reducing agent is:

[0053] (1) Preparation of modified cellulose:

[0054] The cellulose was immersed in a phytic acid solution containing ammonium persulfate for 3 hours (the mass concentration of the phytic acid solution was 20%, and the mass ratio of ammonium persulfate to phytic acid was 1:2), and then dicyanoammonium phosphate was added (the mass ratio of dicyanoammonium phosphate to cellulose was 2:5), and the cellulose was modified by reacting under hydrothermal conditions at 180°C for 10 hours, and then washed and dried to obtain modified cellulose.

[0055] (2) Preparation of polyaniline grafted SiO2:

[0056] S1: dissolving tetraethyl orthosilicate in ethanol, adding ammonium bicarbonate (the mass ratio of tetraethyl orthosilicate, ammonium bicarbonate and ethanol is 1.5:1:40) after sufficient stirring, placing in a hydrothermal reactor after mixing, performing hydrothermal reaction at 160°C for 18h, filtering, washing and drying to prepare SiO2 material;

[0057] S2: Disperse SiO2 material and hexamethylene diisocyanate in acetone, perform ultrasonic dispersion in a nitrogen environment, then add dibutyltin dilaurate (the mass ratio of SiO2 material, hexamethylene diisocyanate, dibutyltin dilaurate, and acetone is 1:1.2:0.01:45), heat to 90°C for reflux reaction for 5 hours, and then filter, wash, and dry to prepare isocyanate SiO2;

[0058] S3: Dissolve isocyanate nano-SiO2 in ethanol, disperse it evenly with ultrasound, then add aniline to react for 3 hours, then add 1 mol / L dilute hydrochloric acid to create an acidic environment (the mass ratio of dilute hydrochloric acid to ethanol is 1:50), then add ammonium persulfate to continue reacting for 8 hours (the mass ratio of isocyanate nano-SiO2, aniline, ammonium persulfate, and ethanol is 1:2:8:45), filter, wash, and dry to prepare polyaniline-grafted SiO2.

[0059] (3) Add EPEG, modified cellulose, polyaniline grafted SiO2 and 150 parts of water into a round-bottom flask and stir thoroughly to dissolve to form a mixed solution A;

[0060] (4) mixing acrylic acid, mercaptoethanol and 80 parts of water, and stirring thoroughly to form a mixed solution B;

[0061] (5) Mix ascorbic acid and 50 parts of water and stir thoroughly to form a mixed solution C;

[0062] (6) Add hydrogen peroxide to mixed solution A, stir for 20 min, and then simultaneously drip into mixed solution B and mixed solution C. The dripping time of mixed solution B is 1 h, and the dripping time of mixed solution C is 1.2 h. After the dripping is completed, the reaction is continued for 1.5 h;

[0063] (7) Adding NaOH solution to the mixed solution obtained in step (6) to control the pH value to 6-8, and then filtering, washing and drying to obtain a gypsum water reducing agent.

[0064] Example 3

[0065] This embodiment provides a gypsum water reducing agent, which is composed of the following raw materials in parts by weight:

[0066] 270 parts of EPEG, 25 parts of acrylic acid, 1 part of mercaptoethanol, 10 parts of modified cellulose, 20 parts of polyaniline grafted SiO2, 0.5 parts of ascorbic acid, 3 parts of 30% hydrogen peroxide, 20 parts of 30% NaOH solution, 300 parts of water;

[0067] The preparation method of the gypsum water reducing agent is:

[0068] (1) Preparation of modified cellulose:

[0069] The cellulose was immersed in a phytic acid solution containing ammonium persulfate for 4 hours (the mass concentration of the phytic acid solution was 20%, and the mass ratio of ammonium persulfate to phytic acid was 1:3), and then dicyanoammonium phosphate was added (the mass ratio of dicyanoammonium phosphate to cellulose was 1:6), and the cellulose was modified by reacting under hydrothermal conditions at 180°C for 10 hours, and then washed and dried to obtain modified cellulose.

[0070] (2) Preparation of polyaniline grafted SiO2:

[0071] S1: dissolving tetraethyl orthosilicate in ethanol, adding ammonium bicarbonate (the mass ratio of tetraethyl orthosilicate, ammonium bicarbonate and ethanol is 2:1:50) after sufficient stirring, placing in a hydrothermal reactor after mixing, performing hydrothermal reaction at 180°C for 20h, filtering, washing and drying to prepare SiO2 material;

[0072] S2: Disperse SiO2 material and hexamethylene diisocyanate in acetone, perform ultrasonic dispersion in a nitrogen environment, then add dibutyltin dilaurate (the mass ratio of SiO2 material, hexamethylene diisocyanate, dibutyltin dilaurate, and acetone is 1:1.5:0.01:50), heat to 80°C for reflux reaction for 6 hours, and then filter, wash, and dry to prepare isocyanate SiO2;

[0073] S3: Dissolve isocyanate nano-SiO2 in ethanol, disperse it evenly with ultrasound, then add aniline to react for 3 hours, then add 1 mol / L dilute hydrochloric acid to create an acidic environment (the mass ratio of dilute hydrochloric acid to ethanol is 1:50), then add ammonium persulfate to continue reacting for 8 hours (the mass ratio of isocyanate nano-SiO2, aniline, ammonium persulfate, and ethanol is 1:2:7:50), filter, wash, and dry to prepare polyaniline-grafted SiO2.

[0074] (3) Add EPEG, modified cellulose, polyaniline-grafted SiO2 and 150 parts of water into a round-bottom flask and stir thoroughly to dissolve to form a mixed solution A;

[0075] (4) mixing acrylic acid, mercaptoethanol and 100 parts of water, and stirring thoroughly to form a mixed solution B;

[0076] (5) Mix ascorbic acid and 50 parts of water and stir thoroughly to form a mixed solution C;

[0077] (6) Add hydrogen peroxide to mixed solution A, stir for 20 min, and then simultaneously drip into mixed solution B and mixed solution C. The dripping time of mixed solution B is 1.1 h, and the dripping time of mixed solution C is 1.2 h. After the dripping is completed, the reaction is continued for 1 h;

[0078] (7) Adding NaOH solution to the mixed solution obtained in step (6) to control the pH value to 6-8, and then filtering, washing and drying to obtain a gypsum water reducing agent.

[0079] Example 4

[0080] This embodiment provides a gypsum water reducing agent, which is composed of the following raw materials in parts by weight:

[0081] 280 parts of EPEG, 30 parts of acrylic acid, 2 parts of mercaptoethanol, 15 parts of modified cellulose, 20 parts of polyaniline grafted SiO2, 1 part of ascorbic acid, 5 parts of 30% hydrogen peroxide, 20 parts of 30% NaOH solution, 300 parts of water;

[0082] The preparation method of the gypsum water reducing agent is:

[0083] (1) Preparation of modified cellulose:

[0084] The cellulose was immersed in a phytic acid solution containing ammonium persulfate for 4 hours (the mass concentration of the phytic acid solution was 10%, and the mass ratio of ammonium persulfate to phytic acid was 1:2), and then dicyanoammonium phosphate was added (the mass ratio of dicyanoammonium phosphate to cellulose was 2:5), and the cellulose was modified by reacting under hydrothermal conditions at 160°C for 12 hours, and then washed and dried to obtain modified cellulose.

[0085] (2) Preparation of polyaniline grafted SiO2:

[0086] S1: dissolving tetraethyl orthosilicate in ethanol, adding ammonium bicarbonate (the mass ratio of tetraethyl orthosilicate, ammonium bicarbonate and ethanol is 1.8:1:48) after sufficient stirring, placing in a hydrothermal reactor after mixing, performing hydrothermal reaction at 160°C for 20h, filtering, washing and drying to prepare SiO2 material;

[0087] S2: Disperse SiO2 material and hexamethylene diisocyanate in acetone, perform ultrasonic dispersion in a nitrogen environment, then add dibutyltin dilaurate (the mass ratio of SiO2 material, hexamethylene diisocyanate, dibutyltin dilaurate, and acetone is 1:1.5:0.015:40), heat to 90°C for reflux reaction for 6 hours, and then filter, wash, and dry to prepare isocyanate SiO2;

[0088] S3: Dissolve isocyanate nano-SiO2 in ethanol, disperse it evenly with ultrasound, then add aniline to react for 3 hours, then add 1 mol / L dilute hydrochloric acid to create an acidic environment (the mass ratio of dilute hydrochloric acid to ethanol is 1:50), then add ammonium persulfate to continue reacting for 8 hours (the mass ratio of isocyanate nano-SiO2, aniline, ammonium persulfate, and ethanol is 1:1.5:7:40), filter, wash, and dry to prepare polyaniline-grafted SiO2.

[0089] (3) Add EPEG, modified cellulose, polyaniline-grafted SiO2 and 150 parts of water into a round-bottom flask and stir thoroughly to dissolve to form a mixed solution A;

[0090] (4) mixing acrylic acid, mercaptoethanol and 100 parts of water, and stirring thoroughly to form a mixed solution B;

[0091] (5) Mix ascorbic acid and 50 parts of water and stir thoroughly to form a mixed solution C;

[0092] (6) Add hydrogen peroxide to mixed solution A, stir for 20 min, and then simultaneously drip into mixed solution B and mixed solution C. The dripping time of mixed solution B is 1.1 h, and the dripping time of mixed solution C is 1.3 h. After the dripping is completed, the reaction is continued for 1.5 h;

[0093] (7) Adding NaOH solution to the mixed solution obtained in step (6) to control the pH value to 6-8, and then filtering, washing and drying to obtain a gypsum water reducing agent.

[0094] Comparative Example 1

[0095] This comparative example provides a gypsum water reducing agent, which is composed of the following raw materials in parts by weight:

[0096] 270 parts of EPEG, 30 parts of acrylic acid, 2 parts of mercaptoethanol, 1 part of ascorbic acid, 5 parts of 30% hydrogen peroxide, 25 parts of 20% NaOH solution, 280 parts of water;

[0097] The preparation method of the gypsum water reducing agent is:

[0098] (1) Add EPEG and 150 parts of water into a round-bottom flask and stir thoroughly to dissolve to form a mixed solution A;

[0099] (2) mixing acrylic acid, mercaptoethanol and 80 parts of water, and stirring thoroughly to form a mixed solution B;

[0100] (3) Mix ascorbic acid and 50 parts of water and stir thoroughly to form a mixed solution C;

[0101] (4) Add hydrogen peroxide to mixed solution A, stir for 20 min, and then simultaneously drip into mixed solution B and mixed solution C. The dripping time of mixed solution B is 1 h, and the dripping time of mixed solution C is 1.2 h. After the dripping is completed, the reaction is continued for 1.5 h;

[0102] (5) Adding NaOH solution to the mixed solution obtained in step (4) to control the pH value to 6-8, and then filtering, washing and drying to obtain a gypsum water reducing agent.

[0103] Comparative Example 2

[0104] This comparative example provides a gypsum water reducing agent, which is composed of the following raw materials in parts by weight:

[0105] 270 parts of EPEG, 30 parts of acrylic acid, 2 parts of mercaptoethanol, 15 parts of modified cellulose, 1 part of ascorbic acid, 5 parts of 30% hydrogen peroxide, 25 parts of 20% NaOH solution, 280 parts of water;

[0106] The preparation method of the gypsum water reducing agent is:

[0107] (1) Preparation of modified cellulose:

[0108] The cellulose was immersed in a phytic acid solution containing ammonium persulfate for 3 hours (the mass concentration of the phytic acid solution was 20%, and the mass ratio of ammonium persulfate to phytic acid was 1:2), and then dicyanoammonium phosphate was added (the mass ratio of dicyanoammonium phosphate to cellulose was 2:5), and the cellulose was modified by reacting under hydrothermal conditions at 180°C for 10 hours, and then washed and dried to obtain modified cellulose.

[0109] (2) Add EPEG, modified cellulose and 150 parts of water into a round-bottom flask and stir thoroughly to dissolve to form a mixed solution A;

[0110] (3) mixing acrylic acid, mercaptoethanol and 80 parts of water, and stirring thoroughly to form a mixed solution B;

[0111] (4) Mix ascorbic acid and 50 parts of water and stir thoroughly to form a mixed solution C;

[0112] (5) Add hydrogen peroxide to mixed solution A, stir for 20 min, and then simultaneously drip into mixed solution B and mixed solution C. The dripping time of mixed solution B is 1 h, and the dripping time of mixed solution C is 1.2 h. After the dripping is completed, the reaction is continued for 1.5 h;

[0113] (6) Adding NaOH solution to the mixed solution obtained in step (5) to control the pH value to 6-8, and then filtering, washing and drying to obtain a gypsum water reducing agent.

[0114] 2 g of the gypsum water-reducing agent prepared in Examples 1 to 4 and Comparative Examples 1 and 2 were respectively weighed and added to 300 g of gypsum and water for stirring, and performance tests were carried out (wherein, the fluidity and compressive strength of the gypsum were tested according to JC / T1023-2021 "Gypsum-based self-leveling mortar", and the water reduction rate was tested according to GB / T 17669.4-1999). The test results are shown in Table 1.

[0115] Table 1

[0116]

Claims

1. A gypsum water reducing agent, characterized in that: The raw material composition includes, by weight: 260-280 parts of EPEG, 20-30 parts of acrylic acid, 1-2 parts of mercaptoethanol, 10-15 parts of modified cellulose, 10-20 parts of polyaniline grafted SiO2, 0.5-1 parts of ascorbic acid, 3-5 parts of hydrogen peroxide, 20-30 parts of NaOH solution, and 250-300 parts of water; The preparation method of the modified cellulose comprises: The cellulose is soaked in a phytic acid solution containing ammonium persulfate for 3-4 hours, and then diammonium phosphate is added to modify the cellulose under hydrothermal conditions, and then the cellulose is washed and dried to obtain modified cellulose. The preparation method of polyaniline grafted SiO2 comprises the following steps: S1: dissolving tetraethyl orthosilicate in ethanol, adding ammonium bicarbonate after sufficient stirring, mixing well and placing in a hydrothermal reactor for hydrothermal reaction, filtering, washing and drying to prepare SiO2 material; S2: Dispersing SiO2 material and hexamethylene diisocyanate in acetone, then adding dibutyltin dilaurate, fully reacting under heating conditions, and then filtering, washing, and drying to prepare isocyanate SiO2; S3: Dissolve isocyanate-treated nano-SiO2 in ethanol, disperse it evenly by ultrasonication, then add aniline to react for 2-3 hours, then drop dilute hydrochloric acid, and then add ammonium persulfate to continue the reaction. After filtering, washing and drying, polyaniline-grafted SiO2 is prepared.

2. The gypsum water reducing agent according to claim 1, characterized in that: The mass concentration of the phytic acid solution is 10-20%, the mass ratio of ammonium persulfate to phytic acid is 1:2-3; the mass ratio of diammonium phosphate to cellulose is 1-2:5-6; After adding diammonium dihydrogen phosphate, the mixture was hydrothermally reacted at 160°C~180°C for 10~12h.

3. The gypsum water reducing agent according to claim 1, characterized in that: In step S1, the mass ratio of ethyl orthosilicate, ammonium bicarbonate and ethanol is 1.5-2:1:40-50; the temperature of the hydrothermal reaction is 160-180° C., and the time is 16-20 hours.

4. The gypsum water reducing agent according to claim 1, characterized in that: In step S2, the mass ratio of SiO2 material, hexamethylene diisocyanate, dibutyltin dilaurate, and acetone is 1:1.2-1.5:0.01-0.015:40-50; After adding dibutyltin dilaurate, heat to 80~90℃ and reflux for 5~6h.

5. The gypsum water reducing agent according to claim 1, characterized in that: In step S2, the SiO2 material and hexamethylene diisocyanate are dispersed in acetone by ultrasonic dispersion in a nitrogen environment.

6. The gypsum water reducing agent according to claim 1, characterized in that: In step S3, the mass ratio of isocyanate nano-SiO2, aniline, ammonium persulfate, and ethanol is 1:1.5-2:6-8:40-50; The concentration of dilute hydrochloric acid is 1 mol / L, and the mass ratio of dilute hydrochloric acid to ethanol is 1:45~50; After adding ammonium persulfate, react for 6 to 8 hours and then filter.

7. The gypsum water reducing agent according to claim 1, characterized in that: The mass fraction of the NaOH solution is 20% to 30%; the mass fraction of the hydrogen peroxide is 30%.

8. The method for preparing a gypsum water reducing agent according to any one of claims 1 to 7, characterized in that: The steps include: (1) Add EPEG, modified cellulose, polyaniline-grafted SiO2 and water into a round-bottom flask and stir thoroughly to dissolve to form a mixed solution A; (2) Mixing acrylic acid, mercaptoethanol and water, and stirring thoroughly to form a mixed solution B; (3) Mix ascorbic acid and water and stir thoroughly to form a mixed solution C; (4) Add hydrogen peroxide to mixed solution A, stir for 10-20 min, then add mixed solution B and mixed solution C dropwise at the same time. After the addition is complete, continue the reaction for 1-1.5 h. (5) Adding NaOH solution to the mixed solution obtained in step (4) to control the pH value to 6-8, and then filtering, washing and drying to obtain a gypsum water reducer.

9. The method for preparing a gypsum water reducing agent according to claim 8, characterized in that: The dropping time of mixed liquid B is 1~1.1h, and the dropping time of mixed liquid C is 1.2~1.3h.

Citation Information

Patent Citations

  • Cellulose / polyaniline nano-porous composite microspheres as well as preparation method and application thereof

    CN104892936A

  • High-strength self-repairing conductive magnetic PVA (Polyvinyl Alcohol) hydrogel and preparation method thereof

    CN107828067A

  • Preparation method of modified cellulose water-retaining agent

    CN112321770A

  • Silicon dioxide modified water reducing agent, phosphogypsum-based self-leveling mortar and preparation method of phosphogypsum-based self-leveling mortar

    CN113912791A