A long afterglow CDs-SiO2 composite material and preparation method thereof
By introducing carbon dots during the silica formation process using a reflow method, a tightly coupled CDs-SiO2 composite material is formed, which solves the problem of weak afterglow signal, achieves long afterglow and nonlinear optical properties, and improves the effect of bioimaging.
Patent Information
- Application Number
- CN202410555656.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-07
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-05-07
AI Technical Summary
In existing technologies, carbon dot and silica composite materials have weak afterglow signals and are difficult to exhibit long afterglow in liquid states. Their nonlinear optical properties are not fully utilized, which limits their application in fields such as bioimaging.
Carbon dots are introduced during the formation of silica using a reflux method, and a tightly coupled CDs-SiO2 composite material is formed in one step to enhance the afterglow signal and introduce delayed fluorescence characteristics, thus achieving efficient long afterglow in both powder and aqueous forms.
It significantly improved the afterglow signal of the composite material, achieved long afterglow performance in both liquid and solid states, and confirmed the two-photon excited fluorescence and photoinduced absorption characteristics, thus improving the effect of bioimaging.
Smart Images

Figure CN118419942B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of materials, and in particular to a long afterglow CDs-SiO2 composite material and a preparation method thereof. Background Art
[0002] Carbon dots (CDs) are smaller than 10 nm in size and belong to a new class of carbon nanomaterials. They have attracted widespread attention since they were first discovered in 2004. CDs have bright light emission and a wide emission range, are easy to prepare, have low / non-toxicity, and are inexpensive to source. They are widely used in fields such as in vitro and in vivo imaging, cancer diagnosis, and biotherapy. The most widely studied photoluminescent property of CDs-based nanomaterials is the common fluorescence, namely single-photon excited fluorescence (1PEF). In the biological spectral window, 1PEF usually exhibits obvious defects in the field of biological imaging, which can be overcome by multiphoton excited fluorescence or phosphorescence imaging. Compared with 1PEF imaging, multiphoton excited fluorescence or phosphorescence imaging exhibits higher resolution, weaker photocytotoxicity, stronger resistance to background / excitation light interference, and deeper penetration depth.
[0003] The nonlinear optical properties of CDs are mainly concentrated in processes such as two-photon absorption (2PA). As the incident light changes to the longer wavelength region, the nonlinear absorption coefficient (αNL) moves to a positive value, indicating that a nonlinear absorption process occurs under a longer ultrafast light source. The corresponding 2PA cross section (σ2PA) can reach 30160GM at 1256nm. In the prior art, a CD whose fluorescence emission intensity is linearly related to the square of the excitation power under ultrafast femtosecond laser excitation is reported, proving the two-photon excited fluorescence (2PEF) property of CDs. Photon induced absorption (PIA) usually occurs in crystals, such as quasi-2D perovskite organic-inorganic single crystals. The formation of the PIA process is due to the electron transition from the lower conduction band to the higher conduction band, and it is different from the normal absorption process usually caused by the electron transition from the valence band to the conduction band. PIA can greatly utilize its excellent performance in fixable holographic recording, which is of great significance to crystals in device applications.
[0004] In view of this, nonlinear optical properties and PIA properties have the above-mentioned advantages, and the development of nanomaterials with these two typical properties deserves more attention. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a long afterglow CDs-SiO2 composite material and a preparation method thereof.
[0006] In a first aspect, the present invention provides a method for preparing a long afterglow CDs-SiO2 composite material, the method for preparing the long afterglow CDs-SiO2 composite material comprising the following steps:
[0007] Powdered carbon dots are obtained;
[0008] Dissolving the powdered carbon dots in water, and then adding tetraethyl orthosilicate and ammonia water to obtain a mixed solution;
[0009] The mixed solution is heated to reflux for reaction to obtain a crude CDs-SiO2 composite material;
[0010] The crude CDs-SiO2 composite material is centrifuged to remove precipitates, and then dialyzed and dried to obtain the long afterglow CDs-SiO2 composite material.
[0011] Furthermore, the step of obtaining powdered carbon dots includes the following process:
[0012] Dissolving polyvinyl alcohol in water, and then mixing with ethylenediamine to obtain a first mixed solution;
[0013] subjecting the first mixed solution to a hydrothermal reaction to obtain a crude reaction product;
[0014] Acetone is added to the crude reaction product to carry out a precipitation reaction, followed by filtration and freeze-drying to obtain the powdered carbon dots.
[0015] Furthermore, the molecular weight of the polyvinyl alcohol is 1000-5000; based on 1g of polyvinyl alcohol, the added amount of ethylenediamine is 0.5-1.0mL.
[0016] Furthermore, the working parameters of the hydrothermal reaction include: temperature of 200-240° C. and time of 8-12 hours.
[0017] Furthermore, the working parameters of the hydrothermal reaction include: temperature of 220° C. and time of 10 h.
[0018] Furthermore, based on 1 mg of the powdered carbon dots, the added amounts of the tetraethyl orthosilicate and the ammonia water are 0.3-0.5 mL and 80-120 μL, respectively.
[0019] Furthermore, the working parameters of the heating reflux reaction include: temperature of 100-110° C. and time of 4-6 hours.
[0020] Furthermore, the working parameters of the heating reflux reaction include: temperature of 100° C. and time of 5 h.
[0021] In a second aspect, the present invention provides a long afterglow CDs-SiO2 composite material, wherein the long afterglow CDs-SiO2 composite material is prepared by the preparation method described in any one of the first aspects.
[0022] The above technical solution provided by the embodiment of the present invention has at least the following advantages compared with the prior art:
[0023] The embodiment of the present invention provides a long afterglow CDs-SiO2 composite material and a preparation method thereof. The present invention introduces carbon dots in the process of gradually forming silicon dioxide by a reflux method, so that the coupling effect between the carbon dots and silicon dioxide is closer, and the embedding effect between the carbon dots and silicon dioxide is more obvious, thereby realizing the preparation of powdery and water-like high-efficiency long afterglow CDs-SiO2 composite materials. Specifically:
[0024] 1) In the prior art, most of the preparation of CDs-SiO2 composite materials is to first synthesize carbon dots and silicon dioxide separately, and then form a composite by reflux method, stirring method or hydrothermal method. The afterglow signal of the obtained composite generally comes from the carbon dots. If the carbon dots before the composite have no afterglow, or the afterglow signal is very weak, the obtained composite will not be significantly improved. However, in this patent, the afterglow signal of the obtained composite is significantly improved compared with that of pure carbon dots. The afterglow signal that can be identified by the naked eye is as long as 20 seconds, and the afterglow signal also triggers the generation of delayed fluorescence signal; before the formation of CDs-SiO2 composite material, the weak afterglow signal of pure carbon dots only comes from the phosphorescent component, and there is no delayed fluorescence component, and the afterglow of pure carbon dots cannot be observed by the naked eye. The "one-step method" involved in the reflux process simultaneously forms a CDs-SiO2 composite material with carbon dots and silicon dioxide, and the CDs-SiO2 composite material exhibits a long afterglow signal in both liquid and solid states, and the afterglow signal after the composite is also significantly improved. The existing reported composite methods only have long afterglow signals in the solid state, and it is difficult to have long afterglow signals in the liquid state.
[0025] 2) The present invention embeds CDs into silica to construct a CDs-SiO2 composite material, achieving efficient and long afterglow in powder and water (including TADF component and phosphorescent component). At the same time, the conversion process from saturated absorption (SA) to anti-saturated absorption was observed when the monitoring light source was a 760nm ultrafast femtosecond laser. The two-photon excited fluorescence (2PEF) characteristics of the CDs-SiO2 composite material have also been successfully confirmed and further applied to biological imaging, which is more conducive to cell imaging compared with 1PEF. In addition, the phosphorescence signal from the CDs-SiO2 composite material was also successfully performed in HeLa cancer cell imaging. In addition, the photoinduced absorption (PIA) phenomenon was observed for the first time in CDs-based nanomaterials by nanosecond transient absorption (ns-TA) spectroscopy, and the detected PIA reached a peak at 466nm, including a "faster component" and a "slower component". CDs-SiO2 can be a good candidate as a saturable absorber or deep tissue imaging agent, with a wide range of practical application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0028] Figure 1 The present invention provides a flow chart of a method for preparing a long afterglow CDs-SiO2 composite material.
[0029] Figure 2 It is a schematic diagram of the assembly process of the CDs-SiO2 composite material of the present invention and the cell imaging of the photoluminescent CDs-SiO2 composite material.
[0030] Figure 3 TEM image of CDs in the present invention.
[0031] Figure 4 This is the TEM image of CDs-SiO2 in the present invention.
[0032] Figure 5 These are photos of CDs-SiO2 powder (top) and CDs-SiO2 solution (bottom) taken under sunlight and 365nm ultraviolet light in the present invention, as well as photos collected within 20 seconds after the light source was turned off.
[0033] Figure 6 It is the UV-visible absorption spectrum of the CDs-SiO2 composite material in the present invention.
[0034] Figure 7 This is the fluorescence spectrum of the CDs-SiO2 composite material in the present invention.
[0035] Figure 8 This is the phosphorescence spectrum of the CDs-SiO2 composite material in the present invention.
[0036] Fig. 9 This is a photoluminescence spectrum of CDs-SiO2 of the CDs-SiO2 composite material in the present invention excited by a 760nm ultrafast femtosecond laser with a power range of 12-80mW.
[0037] Fig.10 It is a Log-Log diagram of the integrated intensity of photoluminescence of the CDs-SiO2 composite material in the present invention versus the power of the excitation light source.
[0038] Fig.11It is a schematic diagram of the 1P / 2P excitation fluorescence process, TADF process and phosphorescence process of the CDs-SiO2 composite material in the present invention.
[0039] Fig.12 The photoluminescence spectra of the CDs-SiO2 composite material of the present invention at 340 nm under different delayed light source durations.
[0040] Fig.13 The normalized fluorescence and phosphorescence spectra of the CDs-SiO2 composite material of the present invention at an excitation wavelength of 340 nm at 80K.
[0041] Fig.14 It is a two-dimensional graph of PL intensity and temperature of the CDs-SiO2 composite material of the present invention.
[0042] Fig.15 This is a temperature-dependent transient PL decay curve of the CDs-SiO2 composite material of the present invention.
[0043] Fig.16 This is a graph showing the average life test results of the CDs-SiO2 composite material of the present invention at different temperatures.
[0044] Fig.17 Figure 2 is the transient absorption spectrum of CDs-SiO2 solution at different time delays.
[0045] Fig.18 The decay traces of CDs-SiO2 solution were detected at 466nm.
[0046] Fig.19 This is the two-photon excitation fluorescence (2PEF) imaging of HeLa cells treated with CDs-SiO2 under 760nm ultrafast femtosecond laser excitation.
[0047] Fig. 20 This is the phosphorescence imaging of HeLa cells by CDs-SiO2 at an excitation wavelength of 340nm. DETAILED DESCRIPTION
[0048] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0050] In the first aspect, the present invention provides a method for preparing a long afterglow CDs-SiO2 composite material, such as Figure 1 As shown, the preparation method of the long afterglow CDs-SiO2 composite material comprises the following steps:
[0051] Powdered carbon dots are obtained;
[0052] Dissolving the powdered carbon dots in water, and then adding tetraethyl orthosilicate and ammonia water to obtain a mixed solution;
[0053] The mixed solution is heated to reflux for reaction to obtain a crude CDs-SiO2 composite material;
[0054] The crude CDs-SiO2 composite material is centrifuged to remove precipitates, and then dialyzed and dried to obtain the long afterglow CDs-SiO2 composite material.
[0055] The embodiment of the present invention provides a method for preparing a long afterglow CDs-SiO2 composite material. The present invention introduces carbon dots in the process of gradually forming silicon dioxide by a reflux method, so that the coupling effect between the carbon dots and silicon dioxide is closer, and the embedding effect between the carbon dots and silicon dioxide is more obvious, thereby realizing the preparation of powdery and water-like high-efficiency long afterglow CDs-SiO2 composite materials. Specifically:
[0056] 1) In the prior art, most of the preparation of CDs-SiO2 composite materials is to first synthesize carbon dots and silicon dioxide separately, and then form a composite by reflux method, stirring method or hydrothermal method. The afterglow signal of the obtained composite generally comes from the carbon dots. If the carbon dots before the composite have no afterglow, or the afterglow signal is very weak, the obtained composite will not be significantly improved. However, in this patent, the afterglow signal of the obtained composite is significantly improved compared with that of pure carbon dots. The afterglow signal that can be identified by the naked eye is as long as 20 seconds, and the afterglow signal also triggers the generation of delayed fluorescence signal. The afterglow signal of carbon dots in the CDs-SiO2 composite material only comes from the phosphorescent component, and there is no delayed fluorescence component, and the afterglow of pure carbon dots cannot be observed by the naked eye. The "one-step method" involved in the reflux process simultaneously forms a CDs-SiO2 composite material with carbon dots and silicon dioxide, and the CDs-SiO2 composite material exhibits a long afterglow signal in both liquid and solid states, and the afterglow signal after the composite is also significantly improved. The existing reported composite methods only have long afterglow signals in the solid state, and it is difficult to have long afterglow signals in the liquid state.
[0057] 2) The present invention embeds CDs into silica to construct a CDs-SiO2 composite material, achieving efficient and long afterglow in powder and water (including TADF component and phosphorescent component). At the same time, the conversion process from saturated absorption (SA) to anti-saturated absorption was observed when the monitoring light source was a 760nm ultrafast femtosecond laser. The two-photon excited fluorescence (2PEF) characteristics of the CDs-SiO2 composite material have also been successfully confirmed and further applied to biological imaging, which is more conducive to cell imaging compared with 1PEF. In addition, the phosphorescence signal from the CDs-SiO2 composite material was also successfully performed in cancer cell imaging. In addition, the photoinduced absorption (PIA) phenomenon was observed in CDs-based nanomaterials for the first time by nanosecond transient absorption (ns-TA) spectroscopy, and the detected PIA reached a peak at 466nm, including a "faster component" and a "slower component". CDs-SiO2 can be a good candidate as a saturable absorber or deep tissue imaging agent, with a wide range of practical application value.
[0058] In some specific embodiments, the step of obtaining powdered carbon dots comprises the following process:
[0059] Dissolving polyvinyl alcohol in water, and then mixing with ethylenediamine to obtain a first mixed solution;
[0060] subjecting the first mixed solution to a hydrothermal reaction to obtain a crude reaction product;
[0061] Acetone is added to the crude reaction product to carry out a precipitation reaction, followed by filtration and freeze-drying to obtain the powdered carbon dots.
[0062] In some specific embodiments, the molecular weight of the polyvinyl alcohol is 1000-5000; based on 1 g of polyvinyl alcohol, the amount of ethylenediamine added is 0.5-1.0 mL.
[0063] In some specific embodiments, the working parameters of the hydrothermal reaction include: temperature of 200-240° C. and time of 8-12 h.
[0064] In some specific embodiments, the working parameters of the hydrothermal reaction include: temperature of 220° C. and time of 10 h.
[0065] In some specific embodiments, based on 1 mg of powdered carbon dots, the added amounts of the tetraethyl orthosilicate and the ammonia water are 0.3-0.5 mL and 80-120 μL, respectively.
[0066] In some specific embodiments, the working parameters of the heating reflux reaction include: temperature of 100-110° C. and time of 4-6 h.
[0067] In some specific embodiments, the working parameters of the heating reflux reaction include: temperature of 100° C. and time of 5 h.
[0068] In a second aspect, based on a general inventive concept, the present invention provides a long afterglow CDs-SiO2 composite material, wherein the long afterglow CDs-SiO2 composite material is prepared by the preparation method described in any one of the first aspects.
[0069] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0070] Example 1
[0071] This example provides a long afterglow CDs-SiO2 composite material, and the preparation method of the long afterglow CDs-SiO2 composite material comprises the following steps:
[0072] Preparation of CDs: 1 g of PVA (polyvinyl alcohol, molecular weight: 1750±50) was dissolved in 20 mL of water, the PVA solution was mixed with 0.75 mL of ethylenediamine, and then transferred into an autoclave for reaction at 220°C for 10 h; after the reaction, the excess PVA was removed by acetone precipitation, the transparent solution was collected and concentrated, and further dialyzed to obtain powdered CDs;
[0073] Preparation of CDs-SiO2 composite material: Pour 5 mg of the prepared carbon dot powder into 10 mL of water and mix well to obtain a carbon dot solution. Then add 2 mL of tetraethyl orthosilicate and 500 μL of ammonia water to the carbon dot solution respectively. Reflux in an oil bath at 100°C for 5 hours to obtain a crude complex of the CDs-SiO2 composite material. Centrifuge to remove the precipitate, dialyze for 2 days to obtain a pure solution of the CDs-SiO2 composite material, and dry at 60°C for 12 hours to obtain a CDs-SiO2 composite material powder.
[0074] Example 2
[0075] This example provides a long afterglow CDs-SiO2 composite material, and the preparation method of the long afterglow CDs-SiO2 composite material comprises the following steps:
[0076] Preparation of CDs: 1 g of PVA (polyvinyl alcohol, molecular weight: 1750±50) was dissolved in 20 mL of water, the PVA solution was mixed with 0.75 mL of ethylenediamine, and then transferred into an autoclave for reaction at 240°C for 8 h; after the reaction, the excess PVA was removed by acetone precipitation, the transparent solution was collected and concentrated, and further dialyzed to obtain powdered CDs;
[0077] Preparation of CDs-SiO2 composite material: Pour 5 mg of the prepared carbon dot powder into 10 mL of water and mix well to obtain a carbon dot solution. Then add 2 mL of tetraethyl orthosilicate and 500 μL of ammonia water to the carbon dot solution respectively. Reflux in an oil bath at 100°C for 5 hours to obtain a crude complex of the CDs-SiO2 composite material. Centrifuge to remove the precipitate, dialyze for 2 days to obtain a pure solution of the CDs-SiO2 composite material, and dry at 60°C for 12 hours to obtain a CDs-SiO2 composite material powder.
[0078] Example 3
[0079] This example provides a long afterglow CDs-SiO2 composite material, and the preparation method of the long afterglow CDs-SiO2 composite material comprises the following steps:
[0080] Preparation of CDs: 1 g of PVA (polyvinyl alcohol, molecular weight: 1750±50) was dissolved in 20 mL of water, the PVA solution was mixed with 0.75 mL of ethylenediamine, and then transferred into an autoclave and reacted at 200°C for 12 h; after the reaction, the excess PVA was removed by acetone precipitation, the transparent solution was collected and concentrated, and further dialyzed to obtain powdered CDs;
[0081] Preparation of CDs-SiO2 composite material: Pour 5 mg of the prepared carbon dot powder into 10 mL of water and mix well to obtain a carbon dot solution. Then add 2 mL of tetraethyl orthosilicate and 500 μL of ammonia water to the carbon dot solution respectively. Reflux in an oil bath at 100°C for 5 hours to obtain a crude complex of the CDs-SiO2 composite material. Centrifuge to remove the precipitate, dialyze for 2 days to obtain a pure solution of the CDs-SiO2 composite material, and dry at 60°C for 12 hours to obtain a CDs-SiO2 composite material powder.
[0082] Test Case
[0083] In this example, the CDs-SiO2 composite material obtained in the above Example 1 was subjected to performance testing and characterization.
[0084] 1) The schematic diagram of the assembly process and cell imaging of the photoluminescent CDs-SiO2 composite material provided by the present invention is as follows Figure 2 As shown. During the assembly process, the weak phosphorescence signal emitted by CDs was continuously enhanced by the denser silica network. At the same time, thermally activated delayed fluorescence (TADF) was observed under UV light. The assembled CDs-SiO2 was incubated into typical human HeLa cancer cells for cell imaging.
[0085] 2) TEM images after hydrothermal reaction show that the diameter of carbon dots (CDs) is about 4 nm. Figure 3After CDs are embedded in nano-silica, the CDs-SiO2 particles formed are quasi-spherical and amorphous, as shown in the high-resolution TEM image ( Figure 4 ). The assembled composite nanoparticles still have a fairly small size of about 20nm, which is beneficial for biomedical applications. Under 365nm handheld UV light, the powdered CDs-SiO2 can emit bright blue light, as shown in Figure 5 As shown. In addition, after the UV source is cut off, the CDs-SiO2 powder exhibits a light green luminescence that can be recognized by the naked eye within 20 seconds and is an afterglow behavior. In addition, the CDs-SiO2 solution also exhibits similar emission behavior as the CDs-SiO2 powder when exposed to UV light and the UV lamp is removed. It is worth mentioning that the afterglow emission is greatly enhanced after the CDs are anchored on the SiO2 shell, because the afterglow from these pure CDs is too weak to be recognized by the human eye. Compared with CDs, TADF emission is also a new phenomenon triggered after the formation of the CDs-SiO2 composite material.
[0086] 3) The normalized spectrum, fluorescence spectrum and phosphorescence spectrum of the CDs-SiO2 composite material of the present invention are respectively as follows: Figure 6 , Figure 7 and Figure 8 As shown; the photoluminescence spectrum of CDs-SiO2 excited by 760nm ultrafast femtosecond laser with a power range of 12-80mW is shown Fig. 9 As shown; the Log-Log diagram of the integrated photoluminescence intensity versus the excitation light source power is shown Fig.10 As shown; the schematic diagram of 1P / 2P excitation fluorescence process, TADF process and phosphorescence process is shown in Fig.11 It shows that the CDs-SiO2 composite material of the present invention successfully exhibits linear optical 1PEF characteristics and nonlinear optical 2PEF characteristics.
[0087] 4) At different delay times, the photoluminescence spectra of the CDs-SiO2 composite material of the present invention at 340 nm are as follows: Fig.12 The normalized fluorescence and phosphorescence spectra of the CDs-SiO2 composite material of the present invention at an excitation wavelength of 340 nm at 80K are shown in FIG. Fig.13 The two-dimensional graph of PL intensity and temperature of the CDs-SiO2 composite material of the present invention is shown in Fig.14 The temperature-dependent transient PL decay curve of the CDs-SiO2 composite material of the present invention (monitored at EM: 418nm, EX: 340nm) is shown in FIG. Fig.15 The average lifespan of the CDs-SiO2 composite material of the present invention (monitored at EM: 418nm, EX: 340nm) at different temperatures is shown in FIG. Fig.16 shown.
[0088] 5) Transient absorption spectra of CDs-SiO2 solution at different time delays are shown in Figure 2 Fig.17 As shown in Figure 2, the photoinduced absorption (PIA) phenomenon of CDs-SiO2 solution was successfully observed by nanosecond transient absorption (ns-TA) spectroscopy, which showed that the PIA peak was at about 466nm after a delay of 10-1000ms in the probe range of 400-800nm. The decay traces of CDs-SiO2 solution were detected at 466nm. Fig.18 As shown, a double exponential function fits the corresponding decay trajectory at 466 nm, which contains a "faster" process and a "slower" process, with decays of 357.4 ms and 8.4 s, respectively.
[0089] 6) Two-photon excitation fluorescence (2PEF) imaging of HeLa cells treated with CDs-SiO2 using 760nm ultrafast femtosecond laser excitation Fig.19 As shown in the figure. The phosphorescence imaging of HeLa cells by CDs-SiO2 at 340nm excitation wavelength is shown in the figure Fig. 20 As shown. Compared with commercial dyes, the CDs-SiO2 prepared by the present invention has advantages in cell imaging. Commercial dyes have disadvantages such as severe photobleaching, poor solubility in water, narrow Stokes shift, complex dyeing process, and high cost. The CDs-SiO2 of the present invention was incubated in HeLa cancer cells for imaging applications. 2PEF imaging signals were collected under 760nm ultrafast femtosecond laser excitation, as shown Fig.19 As shown in Figures ac, the fluorescence signal is bright. The present invention also explores the potential of phosphorescence imaging, such as Fig. 20 As shown in Figures ac, the phosphorescence signal was also captured after the composite was excited with a 340 nm light source. It is worth noting that the CDs-SiO2 composite stained HeLa cells for only 20 min, and the obvious photoluminescence signal could be well dispersed in the cytoplasm region, indicating that the CDs-SiO2 composite could easily penetrate the cell membrane and enter the cancer cells. These properties indicate that the CDs-SiO2 composite has good cell penetration ability. Therefore, the CDs-SiO2 composite can be an excellent candidate for cell imaging.
[0090] Through the above tests, it can be known that: the present invention embeds CDs into silica to construct a CDs-SiO2 composite material, and realizes powder and water-like efficient long afterglow (including TADF component and phosphorescent component). At the same time, when the monitoring light source is a 760nm ultrafast femtosecond laser, the conversion process from saturated absorption (SA) to anti-saturated absorption is observed. The two-photon excited fluorescence (2PEF) characteristics of the CDs-SiO2 composite material have also been successfully confirmed and further applied to biological imaging, which is more conducive to cell imaging compared with 1PEF. In addition, the phosphorescence signal from the CDs-SiO2 composite material has also been successfully performed in cancer cell imaging. In addition, the photoinduced absorption (PIA) phenomenon was observed in CDs-based nanomaterials for the first time by nanosecond transient absorption (ns-TA) spectroscopy, and the detected PIA reached a peak at 466nm, including "faster components" and "slower components". CDs-SiO2 can be a good candidate as a saturable absorber or deep tissue imaging agent, and has a wide range of practical application value.
[0091] Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0092] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for preparing a long afterglow CDs-SiO2 composite material, characterized in that: The long afterglow CDs-SiO2 composite material has linear optical properties, nonlinear optical properties, light-induced absorption properties and thermally activated delayed fluorescence properties; the preparation method of the long afterglow CDs-SiO2 composite material comprises the following steps: Powdered carbon dots are obtained; Dissolving the powdered carbon dots in water, and then adding tetraethyl orthosilicate and ammonia water to obtain a mixed solution; The mixed solution is heated to reflux for reaction to obtain a crude CDs-SiO2 composite material; Centrifuging the crude CDs-SiO2 composite material to remove precipitates, then dialyzing and drying to obtain the long afterglow CDs-SiO2 composite material; Based on 1 mg of powdered carbon dots, the added amounts of the tetraethyl orthosilicate and the ammonia water are 0.3-0.5 mL and 80-120 μL, respectively; The working parameters of the heating reflux reaction include: temperature of 100-110° C. and time of 4-6 hours.
2. The method for preparing the long afterglow CDs-SiO2 composite material according to claim 1, characterized in that: The steps to obtain powdered carbon dots include the following processes: Dissolving polyvinyl alcohol in water, and then mixing with ethylenediamine to obtain a first mixed solution; subjecting the first mixed solution to a hydrothermal reaction to obtain a crude reaction product; Acetone is added to the crude reaction product to carry out a precipitation reaction, followed by filtration and freeze-drying to obtain the powdered carbon dots.
3. The method for preparing the long afterglow CDs-SiO2 composite material according to claim 2, characterized in that: The molecular weight of the polyvinyl alcohol is 1000-5000; based on 1g of polyvinyl alcohol, the added amount of ethylenediamine is 0.5-1.0mL.
4. The method for preparing the long afterglow CDs-SiO2 composite material according to claim 2, characterized in that: The working parameters of the hydrothermal reaction include: temperature of 200-240° C. and time of 8-12 hours.
5. The method for preparing the long afterglow CDs-SiO2 composite material according to claim 2, characterized in that: The working parameters of the hydrothermal reaction include: temperature of 220° C. and time of 10 h.
6. The method for preparing the long afterglow CDs-SiO2 composite material according to claim 1, characterized in that: The working parameters of the heating reflux reaction include: temperature of 100° C. and time of 5 h.
7. A long afterglow CDs-SiO2 composite material, characterized in that: The long afterglow CDs-SiO2 composite material is prepared by the preparation method described in any one of claims 1 to 6.