A method for preparing a wear-resistant water-based coating

By using polyether modified polyacrylonitrile fibers and carbon chloride nanotubes in aqueous epoxy resin coatings, the problem of insufficient toughness and wear resistance of the coating is solved, and its bending strength, impact strength and wear resistance are significantly improved. Achieve better performance improvements.

CN118421168BActive Publication Date: 2024-12-06DONGGUAN WUREN NEW MATERIAL TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410672547.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-28
Publication Date
2024-12-06
Estimated Expiration
2044-05-28

AI Technical Summary

Technical Problem

The toughness and poor wear resistance of water-based epoxy resin coatings limit their development and application in wear-resistant coatings.

Method used

Polyether modified polyacrylonitrile fibers and carbon acyl chloride nanotubes are used as the main fillers to modify the fiber surface through acrylamide polyether graft reaction, increasing the hydrophilicity and flexible segments of the fiber, and modifying carbon by acid chloride Nanotubes improve their dispersion and interface bonding properties in epoxy resins, and improve the toughness and wear resistance of the coating.

Benefits of technology

The bending strength, impact strength and wear resistance of the aqueous epoxy resin are significantly improved, the friction coefficient is reduced, and the overall performance of the coating is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004863094140000041
    Figure BDA0004863094140000041
  • Figure BDA0004863094140000071
    Figure BDA0004863094140000071
Patent Text Reader

Abstract

The invention discloses a method for preparing a wear-resistant water-based coating. The acrylamide-based polyether of the invention undergoes a grafting reaction on the surface of a polyacrylonitrile fiber under the action of dibenzoyl peroxide to obtain a polyether-modified polyacrylonitrile fiber. The polyether-modified polyacrylonitrile fiber and the chlorinated carbon nanotubes are used as the main fillers of the water-based epoxy resin. The polyether-modified polyacrylonitrile fiber and the epoxy resin have better interface bonding performance, and the carbon nanotubes are modified on the surface of the polyether-modified polyacrylonitrile fiber to have better dispersibility. During the friction process of the epoxy resin, the friction force generated can be effectively transmitted to the polyacrylonitrile fiber and the carbon nanotubes, reducing the stress concentration of the epoxy resin and preventing crack extension, thereby improving the wear resistance of the epoxy resin and showing a lower friction coefficient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, in particular to a method for preparing a wear-resistant water-based coating. Background Art

[0002] Polyacrylonitrile fiber has the advantages of high strength, high modulus, and simple preparation method. It is a fiber material with excellent comprehensive performance and can be used in materials such as coatings, foams, and concrete to improve the toughness, strength and other properties of the materials. The surface affinity and hydrophilicity of polyacrylonitrile fiber can be improved by grafting polyacrylonitrile fiber with olefin-containing monomers.

[0003] As a nanomaterial with excellent performance, carbon nanotubes are widely used in polymer materials such as epoxy resin, polystyrene, and rubber. The research focus is on surface modification of carbon nanotubes, improving their compatibility with polymer materials, and overcoming the agglomeration problem of carbon nanotubes. Waterborne epoxy resin coatings are green and environmentally friendly, with little pollution. Although they have good insulation and anti-corrosion properties, waterborne epoxy resins have poor toughness and poor wear resistance, which hinders the development and application of epoxy resins in wear-resistant coatings. It is necessary to improve the toughness, wear resistance and other properties of waterborne epoxy resin coatings. Summary of the invention

[0004] The invention solves the problem that the water-based epoxy resin coating has poor toughness and poor wear resistance.

[0005] The technical scheme of the present invention is: a wear-resistant water-based paint, comprising 92-98.5 parts by weight of water-based epoxy resin, 1-6 parts by weight of polyether-modified polyacrylonitrile fiber, 0.5-2 parts by weight of acyl chloride carbon nanotubes, 0.3-0.6 parts by weight of defoamer, and 0.2-0.4 parts by weight of leveling agent.

[0006] Further, the preparation method of polyether modified polyacrylonitrile fiber is as follows:

[0007] Step (1), adding polyethylene glycol monomethyl ether glycidyl ether, N-(3-aminopropyl)methacrylamide hydrochloride and triethylamine in a molar ratio of 1:(1.4-1.8):(1.5-2) to N,N-dimethylformamide, stirring to react, removing N,N-dimethylformamide by distillation under reduced pressure, adding the product to diethyl ether to precipitate, filtering and drying to obtain acrylamide polyether.

[0008] Step (2), adding acrylamide polyether and dibenzoyl peroxide to distilled water, stirring to dissolve, and then adding polyacrylonitrile fiber, stirring, and then carrying out grafting reaction at 70-85° C. for 3-5 hours, filtering, washing with distilled water and acetone in sequence, and drying to obtain polyether-modified polyacrylonitrile fiber.

[0009] Furthermore, the reaction in step (1) is carried out at 70-90° C. for 12-18 h.

[0010] Furthermore, in step (2), the mass ratio of acrylamide polyether, dibenzoyl peroxide and polyacrylonitrile fiber is (5-40):(0.004-0.03):100.

[0011] Furthermore, the preparation method of chlorinated carbon nanotubes is: adding carbon nanotubes to concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1 for oxidation; then adding the oxidized carbon nanotubes to a mixed solution of thionyl chloride and N,N-dimethylformamide for chlorination to obtain chlorinated carbon nanotubes.

[0012] Furthermore, the preparation method of the wear-resistant water-based coating is as follows: 1-6 parts by weight of polyether modified polyacrylonitrile fiber and 0.5-2 parts by weight of acyl chloride carbon nanotubes are added to N,N-dimethylformamide, and after dispersion, the mixture is stirred and reacted at room temperature for 6-12 hours, and N,N-dimethylformamide is removed by vacuum distillation. After washing with distilled water, the product is added to 92-98.5 parts by weight of water-based epoxy resin, and finally 0.3-0.6 parts by weight of a defoaming agent and 0.2-0.4 parts by weight of a leveling agent are added, and high-speed shearing is performed to obtain the wear-resistant water-based coating.

[0013] The technical effect of the present invention is as follows: the present invention utilizes polyethylene glycol monomethyl ether glycidyl ether and N-(3-aminopropyl) methacrylamide hydrochloride to undergo a ring-opening reaction to obtain an acrylamide-based polyether containing an alkenyl group, and under the action of dibenzoyl peroxide, a grafting reaction occurs on the surface of polyacrylonitrile fiber to obtain a polyether-modified polyacrylonitrile fiber.

[0014] The present invention uses polyether-modified polyacrylonitrile fiber and chlorinated carbon nanotubes as main fillers of water-based epoxy resin. The polyether flexible chain segments grafted onto the polyacrylonitrile fiber have a good toughening effect on the epoxy resin. The polyacrylonitrile fiber itself also has high mechanical properties such as bending strength and modulus. The grafted polyether chain segments have good hydrophilicity and can improve the dispersibility of the fiber in the epoxy resin aqueous emulsion, thereby enabling the polyacrylonitrile fiber to exert a better toughening effect and significantly improving the bending strength and impact strength of the epoxy resin.

[0015] The acrylamide polyether prepared by the invention contains imino groups and hydroxyl groups. The acrylamide polyether is grafted onto the surface of polyacrylonitrile fiber, thereby introducing imino groups and hydroxyl active groups onto the fiber surface, which can undergo amidation and esterification reactions with the acyl chloride groups of acyl chloride carbon nanotubes, thereby bonding the polyether-modified polyacrylonitrile fiber to the surface of the carbon nanotubes, thereby realizing surface modification of the carbon nanotubes. After the surface modification, the carbon nanotubes are added into the waterborne epoxy resin, thereby improving the agglomeration problem of the carbon nanotubes, making the carbon nanotubes uniformly dispersed in the epoxy resin, and further enhancing the bending strength, impact strength and toughness of the epoxy resin.

[0016] The polyether-modified polyacrylonitrile fiber of the present invention has better interface bonding performance with the epoxy resin, and the carbon nanotubes are surface-modified by the polyether-modified polyacrylonitrile fiber and have better dispersibility. During the friction process of the epoxy resin, the friction force generated can be effectively transferred to the polyacrylonitrile fiber and the carbon nanotubes, reducing the stress concentration of the epoxy resin and preventing crack propagation, thereby improving the wear resistance of the epoxy resin and showing a lower friction coefficient. DETAILED DESCRIPTION

[0017] The waterborne epoxy resin of the present invention has a brand number of EP137 and a solid content of 52%.

[0018] Polyacrylonitrile fiber model AF60.

[0019] 0.5 g of carbon nanotubes were added to 210 mL of concentrated sulfuric acid and 70 mL of concentrated nitric acid, ultrasonically treated at 40°C for 4 h, diluted with distilled water, filtered with a cellulose microporous membrane, washed with distilled water, and dried to obtain oxidized carbon nanotubes; then placed in 50 mL of thionyl chloride, 10 mL of N,N-dimethylformamide was added, reacted at 60°C for 48 h, centrifuged, washed with tetrahydrofuran, and dried to obtain chlorinated carbon nanotubes.

[0020] Add 5mmol of polyethylene glycol monomethyl ether 2000 to 50mL of toluene, add 7.5mmol of sodium hydride, react at 30℃ for 2h, then add 20mmol of epichlorohydrin, react at 40℃ for 6h, add ether for precipitation, filter, dissolve the product in dichloromethane, add distilled water for extraction and washing, collect the dichloromethane organic phase, add ether for precipitation, filter, and obtain polyethylene glycol monomethyl ether glycidyl ether. The structural formula is

[0021] Example 1

[0022] Add 10mmol of polyethylene glycol monomethyl ether glycidyl ether, 18mmol of N-(3-aminopropyl) methacrylamide hydrochloride, and 18mmol of triethylamine to 150mL of N,N-dimethylformamide, stir and react at 80°C for 12h, remove N,N-dimethylformamide by vacuum distillation, add the product to ether to precipitate, filter, and dry to obtain acrylamide polyether. The reaction formula is:

[0023]

[0024] Add 2.5 g acrylamide polyether and 2 mg dibenzoyl peroxide to 200 mL distilled water, stir to dissolve, then add 50 g polyacrylonitrile fiber, stir and carry out grafting reaction at 70°C for 3 h, filter, wash with distilled water and acetone in turn, and dry to obtain polyether modified polyacrylonitrile fiber.

[0025] 1 g of polyether modified polyacrylonitrile fiber and 0.5 g of acyl chloride carbon nanotubes were added to 15 mL of N, N-dimethylformamide, and the mixture was stirred and reacted at room temperature for 6 h after dispersion. N, N-dimethylformamide was removed by vacuum distillation. The product was washed with distilled water and added to 98.5 g of water-based epoxy resin. Finally, 0.6 g of defoamer TEGO-8030 and 0.3 g of leveling agent BYK381 were added, and the mixture was sheared at high speed to obtain a wear-resistant water-based coating.

[0026] Example 2

[0027] To 150 mL of N,N-dimethylformamide, add 10 mmol of polyethylene glycol monomethyl ether glycidyl ether, 14 mmol of N-(3-aminopropyl)methacrylamide hydrochloride, and 20 mmol of triethylamine, stir and react at 70°C for 15 h, remove N,N-dimethylformamide by distillation under reduced pressure, add the product to diethyl ether to precipitate, filter, and dry to obtain acrylamide polyether.

[0028] Add 4 g acrylamide polyether and 6 mg dibenzoyl peroxide to 300 mL distilled water, stir to dissolve, then add 50 g polyacrylonitrile fiber, stir and carry out grafting reaction at 70°C for 5 h, filter, wash with distilled water and acetone in turn, and dry to obtain polyether modified polyacrylonitrile fiber.

[0029] 2.5 g of polyether modified polyacrylonitrile fiber and 1 g of acyl chloride carbon nanotubes were added to 30 mL of N, N-dimethylformamide, and the mixture was stirred and reacted at room temperature for 6 h after dispersion. N, N-dimethylformamide was removed by vacuum distillation. The product was washed with distilled water and added to 96.5 g of water-based epoxy resin. Finally, 0.6 g of defoamer TEGO-8030 and 0.2 g of leveling agent BYK381 were added, and the mixture was sheared at high speed to obtain a wear-resistant water-based coating.

[0030] Example 3

[0031] To 200 mL of N,N-dimethylformamide, 10 mmol of polyethylene glycol monomethyl ether glycidyl ether, 15 mmol of N-(3-aminopropyl)methacrylamide hydrochloride, and 20 mmol of triethylamine were added, and the mixture was stirred at 90°C for 12 h. N,N-dimethylformamide was removed by distillation under reduced pressure, and the product was added to diethyl ether to precipitate, which was filtered and dried to obtain acrylamide polyether.

[0032] Add 6 g of acrylamide polyether and 10 mg of dibenzoyl peroxide to 300 mL of distilled water, stir to dissolve, then add 50 g of polyacrylonitrile fiber, stir and carry out grafting reaction at 80°C for 4 hours, filter, wash with distilled water and acetone in turn, and dry to obtain polyether-modified polyacrylonitrile fiber.

[0033] 4.5 g of polyether modified polyacrylonitrile fiber and 1.5 g of acyl chloride carbon nanotubes were added to 50 mL of N, N-dimethylformamide, and the mixture was stirred and reacted at room temperature for 12 h after dispersion. N, N-dimethylformamide was removed by distillation under reduced pressure. The product was washed with distilled water and added to 94 g of water-based epoxy resin. Finally, 0.3 g of defoamer TEGO-8030 and 0.4 g of leveling agent BYK381 were added, and the mixture was sheared at high speed to obtain a wear-resistant water-based coating.

[0034] Example 4

[0035] To 150 mL of N,N-dimethylformamide, 10 mmol of polyethylene glycol monomethyl ether glycidyl ether, 14 mmol of N-(3-aminopropyl)methacrylamide hydrochloride, and 15 mmol of triethylamine were added, and the mixture was stirred at 70°C for 18 h. N,N-dimethylformamide was removed by distillation under reduced pressure, and the product was added to diethyl ether to precipitate, which was filtered and dried to obtain acrylamide polyether.

[0036] Add 8 g of acrylamide polyether and 15 mg of dibenzoyl peroxide to 300 mL of distilled water, stir to dissolve, then add 50 g of polyacrylonitrile fiber, stir and carry out grafting reaction at 85°C for 3 hours, filter, wash with distilled water and acetone in turn, and dry to obtain polyether-modified polyacrylonitrile fiber.

[0037] 6 g of polyether modified polyacrylonitrile fiber and 2 g of acyl chloride carbon nanotubes were added to 80 mL of N, N-dimethylformamide, and the mixture was stirred and reacted at room temperature for 12 h after dispersion. N, N-dimethylformamide was removed by vacuum distillation. The product was washed with distilled water and added to 92 g of water-based epoxy resin. Finally, 0.3 g of defoamer TEGO-8030 and 0.3 g of leveling agent BYK381 were added, and the mixture was sheared at high speed to obtain a wear-resistant water-based coating.

[0038] Comparative Example 1

[0039] 0.6 g of defoamer TEGO-8030 and 0.3 g of leveling agent BYK381 were added to 98.5 g of water-based epoxy resin, and sheared at high speed to obtain a wear-resistant water-based coating.

[0040] Comparative Example 2

[0041] 1 g of polyether-modified polyacrylonitrile fiber was added to 98.5 g of water-based epoxy resin, and finally 0.6 g of defoamer TEGO-8030 and 0.3 g of leveling agent BYK381 were added, and high-speed shearing was performed to obtain a wear-resistant water-based coating.

[0042] Comparative Example 3

[0043] 0.5 g of acyl chloride carbon nanotubes was added to 98.5 g of water-based epoxy resin, and finally 0.6 g of defoamer TEGO-8030 and 0.3 g of leveling agent BYK381 were added, and high-speed shearing was performed to obtain a wear-resistant water-based coating.

[0044] Comparative Example 4

[0045] 1 g of polyether modified polyacrylonitrile fiber and 0.5 g of carbon nanotubes were added to 15 mL of N, N-dimethylformamide, and the mixture was stirred at room temperature for 6 h after dispersion. N, N-dimethylformamide was removed by distillation under reduced pressure. The product was washed with distilled water and added to 98.5 g of water-based epoxy resin. Finally, 0.6 g of defoamer TEGO-8030 and 0.3 g of leveling agent BYK381 were added, and the mixture was sheared at high speed to obtain a wear-resistant water-based coating.

[0046] Comparative Example 5

[0047] 1 g of polyacrylonitrile fiber and 0.5 g of acyl chloride carbon nanotubes were added to 15 mL of N,N-dimethylformamide, and the mixture was stirred at room temperature for 6 h after dispersion. N,N-dimethylformamide was removed by distillation under reduced pressure. The product was washed with distilled water and added to 98.5 g of water-based epoxy resin. Finally, 0.6 g of defoamer TEGO-8030 and 0.3 g of leveling agent BYK381 were added, and the mixture was sheared at high speed to obtain a wear-resistant water-based coating.

[0048] 22g of polyamide 651 curing agent was added to the wear-resistant water-based coating, and the coating was cured at 100°C for 4h and 140°C for 2h to obtain an epoxy resin sample. The bending and impact properties were tested according to the method of GB / T2567-2008.

[0049] Wear resistance test: refer to GB / T 3960-2016 standard, use wear testing machine for testing, load is 200N, test time is 60min, 45# steel ring is used as the wear part, and the friction coefficient is tested.

[0050] Table 1 Performance test of wear-resistant water-based coatings

[0051]

[0052] As shown in Table 1, the flexural strength of the wear-resistant water-based coatings of Examples 1-4 reached 135.9-158.3 MPa, and the impact strength reached 18.3-27.0 kJ / m 2 , the friction coefficient is only 0.486-0.553%, showing good toughness and wear resistance. This is because the polyether flexible chain segment grafted on the polyacrylonitrile fiber has a good toughening effect on the epoxy resin. At the same time, the polyacrylonitrile fiber itself also has high mechanical properties such as bending strength and modulus. The grafted polyether chain segment has good hydrophilicity, which can improve the dispersion of the fiber in the epoxy resin aqueous emulsion, so that the polyacrylonitrile fiber can play a better toughening effect and significantly improve the bending strength and impact strength of the epoxy resin.

[0053] Acrylamide polyether contains imino and hydroxyl groups. Acrylamide polyether is grafted onto the surface of polyacrylonitrile fiber, thereby introducing imino and hydroxyl active groups on the fiber surface, which can react with the acyl chloride groups of acyl chloride carbon nanotubes, thereby bonding the polyether-modified polyacrylonitrile fiber to the surface of the carbon nanotubes, thereby realizing the surface modification of the carbon nanotubes. After the surface modification, the carbon nanotubes are added to the water-based epoxy resin, which can improve the agglomeration problem of the carbon nanotubes, make the carbon nanotubes evenly dispersed in the epoxy resin, and further enhance the bending strength, impact strength and toughness of the epoxy resin.

[0054] There is better interface bonding performance between polyether modified polyacrylonitrile fiber and epoxy resin, and carbon nanotubes are better dispersed after being surface modified by polyether modified polyacrylonitrile fiber. During the friction process of epoxy resin, the friction force generated can be effectively transferred to the polyacrylonitrile fiber and carbon nanotubes, reducing the stress concentration of epoxy resin and preventing crack propagation, thereby improving the wear resistance of epoxy resin and showing a lower friction coefficient.

[0055] Compared with Example 1, polyether-modified polyacrylonitrile fibers and carbon nanotubes are added to the epoxy resin of Comparative Example 4. The carbon nanotubes do not contain acyl chloride groups and cannot react with the imino and hydroxyl groups of the polyether-modified polyacrylonitrile fibers, resulting in the polyether-modified polyacrylonitrile fibers not being modified on the surface of the carbon nanotubes. When added to the epoxy resin, the carbon nanotubes are easily agglomerated, resulting in the bending strength and impact strength of the epoxy resin being lower than those in Example 1, and a larger friction coefficient.

[0056] Compared with Example 1, polyacrylonitrile fibers and chlorinated carbon nanotubes are added to the epoxy resin of Comparative Example 4, but no acrylamide polyether is added to the polyacrylonitrile fibers, and no hydrophilic polyether flexible chain segments are grafted on the surface. The fibers do not contain amino groups or hydroxyl groups, and thus cannot react with chlorinated carbon nanotubes. The carbon nanotubes are not surface modified, resulting in lower bending strength and impact strength of the epoxy resin than those in Example 1, and a larger friction coefficient.

Claims

1. A wear-resistant water-based coating, characterized in that: The wear-resistant water-based coating comprises 92-98.5 parts by weight of water-based epoxy resin, 1-6 parts by weight of polyether-modified polyacrylonitrile fiber, 0.5-2 parts by weight of acyl chloride carbon nanotubes, 0.3-0.6 parts by weight of defoamer, and 0.2-0.4 parts by weight of leveling agent; The preparation method of the polyether-modified polyacrylonitrile fiber is as follows: Step (1), adding polyethylene glycol monomethyl ether glycidyl ether, N-(3-aminopropyl) methacrylamide hydrochloride and triethylamine to N,N-dimethylformamide, stirring to react, removing N,N-dimethylformamide by distillation under reduced pressure, adding the product to diethyl ether to precipitate, filtering and drying to obtain acrylamide polyether; Step (2), adding acrylamide polyether and dibenzoyl peroxide to distilled water, stirring to dissolve, then adding polyacrylonitrile fiber, stirring to carry out grafting reaction, filtering, washing with distilled water and acetone in sequence, and drying to obtain polyether-modified polyacrylonitrile fiber; In the step (1), the molar ratio of polyethylene glycol monomethyl ether glycidyl ether, N-(3-aminopropyl)methacrylamide hydrochloride, and triethylamine is 1:(1.4-1.8):(1.5-2); The reaction in step (1) is carried out at 70-90° C. for 12-18 hours; In the step (2), the mass ratio of acrylamide polyether, dibenzoyl peroxide and polyacrylonitrile fiber is (5-40):(0.004-0.03):100; The grafting reaction in step (2) is carried out at 70-85° C. for 3-5 hours; The preparation method of the chlorinated carbon nanotubes comprises: adding the carbon nanotubes to concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1 for oxidation; then adding the oxidized carbon nanotubes to a mixed solution of thionyl chloride and N,N-dimethylformamide for chlorination to obtain chlorinated carbon nanotubes.

2. A method for preparing a wear-resistant water-based coating as claimed in claim 1, characterized in that: The preparation method is as follows: 1-6 parts by weight of polyether modified polyacrylonitrile fiber and 0.5-2 parts by weight of acyl chloride carbon nanotubes are added to N,N-dimethylformamide, and after dispersion, the mixture is stirred and reacted at room temperature for 6-12 hours, and the N,N-dimethylformamide is removed by vacuum distillation. After washing with distilled water, the product is added to 92-98.5 parts by weight of waterborne epoxy resin, and finally 0.3-0.6 parts by weight of a defoamer and 0.2-0.4 parts by weight of a leveling agent are added, and high-speed shearing is performed to obtain a wear-resistant waterborne coating.

Citation Information

Patent Citations

  • Epoxy mortar adopting surface modified fibers for toughness enhancement

    CN106517959A

  • Toughening epoxy resin composite material as well as preparation and application thereof

    CN110343364A

  • Super-wear-resistant toughened modified water-borne epoxy resin floor paint and preparation method thereof