A method for preparing a heterojunction using a controllable pressure gradient
By designing a controllable pressure gradient on the diamond anvil device and using different solid pressure transmission media to form low-pressure and high-pressure areas, the existing problems of high cost and cumbersome process of heterojunction preparation are solved, and a portable, cheap and efficient Heterojunction preparation, suitable for a variety of device applications.
Patent Information
- Application Number
- CN202410532021.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-04-29
AI Technical Summary
Existing heterojunction preparation methods are costly and cumbersome, and the uncontrollable pressure gradient in the diamond anvil device results in uneven sample structures, making it difficult to implement device applications.
Designing a diamond anvil device with controllable pressure gradient, using different solid pressure-transmitting media on the anvil surface to form a pressure gradient, so that both ends of the sample are located in low-pressure and high-pressure areas respectively. Ruby powder is used to calibrate the pressure distribution to ensure that the sample is in the high-pressure area. A phase change occurs, thereby achieving the construction of a heterostructure.
It realizes the portable, cheap and efficient preparation of heterojunctions, and can quickly prepare various types of heterojunction devices at room temperature. It is suitable for rectification devices and photoelectric detection and other fields, and has good rectification and photoelectric properties.
Smart Images

Figure CN118437229B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of heterojunction preparation, and in particular to a method for preparing a heterojunction by utilizing a controllable pressure gradient. Background Art
[0002] Heterojunctions are usually composed of two or more different materials. Due to their different energy band structures, potential barriers are generated at the interface, thus having rectification and switching characteristics. In addition, due to their excellent optoelectronic properties, they have received extensive attention in research fields such as transistors, solar cells, photocatalysis, photodetection, and lasers in recent years. The current methods for preparing heterojunctions mainly include molecular beam epitaxy, chemical vapor transport, physical vapor transport, solution processing, transfer technology, self-assembly, and photolithography. High-quality heterojunctions usually require high preparation costs and cumbersome preparation processes, so it is of great significance to develop new, portable, and inexpensive preparation processes.
[0003] The Diamond Anvil Cell (DAC) is a portable experimental device used to generate an extremely high-pressure environment. By placing two diamonds close to each other to generate a pressure of one million atmospheres in a space of hundreds of microns, the structure and properties of materials can be regulated. It has been widely used in research fields such as materials science, geology, physics, and chemistry. Under the action of one million atmospheres of pressure, materials usually undergo structural phase transitions due to drastic changes in bond lengths and bond angles, and their physical and chemical properties also change accordingly. With the help of DAC, people have discovered a series of novel and important physical and chemical phenomena, including hydrogen-rich superconductivity, piezoluminescence, metallization, and changes in carrier types. However, at this stage, people mainly use DAC to focus on basic research on materials, and how to realize the practical application of devices is also one of the problems to be solved.
[0004] There is an uncontrollable pressure gradient from the center to the edge of the DAC anvil, with the highest pressure in the center and the lowest at the edge. In order to avoid the inhomogeneity of the pressure gradient on the sample to be tested, researchers usually use gas or liquid pressure transmission media to put the sample in a hydrostatic or quasi-hydrostatic environment. However, if a controllable pressure gradient can be designed on the anvil surface and applied to both ends of the same sample, considering the possible metallization and carrier type changes that may occur when the material undergoes phase change, it is possible to realize different types of self-heterojunction devices in situ in the pressure chamber. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a heterojunction using a controllable pressure gradient. By designing a controllable pressure gradient on the anvil surface of a diamond anvil device, the two ends of the sample are respectively located in a low-pressure area and a high-pressure area, and pressurization causes a phase change in the sample in the high-pressure area to achieve the construction of a heterojunction.
[0006] The specific steps include:
[0007] S1. Gasket preparation; design and specify two area shapes to be filled with the first type of solid pressure transmission medium and the second type of solid pressure transmission medium, the first type of solid pressure transmission medium and the second type of solid pressure transmission medium are two different types of solid pressure transmission medium, and a pressure gradient is formed between the two areas during compression; calibrate the pressure distribution on the diamond anvil surface by ruby powder to confirm the formation of a controllable pressure gradient;
[0008] S2. Select a sample; place the sample at the center of the anvil surface, with the two ends located in the areas where two different types of solid pressure-transmitting media are located; place a ruby ball at each end of the sample for subsequent pressure calibration; and connect wires at both ends of the sample for subsequent photoelectric property measurements;
[0009] S3. Pressurize the device; cause the sample in the area where the first type of solid pressure transmission medium is located to undergo a structural phase change, and ensure that the sample in the area where the second type of solid pressure transmission medium is located still maintains the initial structure, that is, the pressure in the area where the second type of solid pressure transmission medium is located is lower than the pressure required for phase change through ruby calibration; at this time, the sample forms a heterogeneous structure with two ends of a low-pressure phase and a high-pressure phase.
[0010] Preferably, the first type of solid pressure transmission medium and the second type of solid pressure transmission medium of the present invention are cubic boron nitride cBN and sodium chloride NaCl, respectively. A regular shape is cut out of the cBN region and filled with NaCl. Due to the difference in bulk modulus of cBN and NaCl when compressed, a certain pressure gradient is formed between the two regions when compressed.
[0011] The heterojunction obtained by the preparation method described above can realize various types of heterojunctions, including:
[0012] If the low-voltage phase is an n / p-type semiconductor, the high-voltage phase is still an n / p-type semiconductor, which is a heterojunction of the same type of semiconductor;
[0013] If the low-voltage phase is an n / p-type semiconductor and the high-voltage phase is a p / n-type semiconductor, it is an inversion semiconductor heterojunction, i.e., a pn junction;
[0014] If the low-voltage phase is an n / p-type semiconductor and the high-voltage phase is a metal, it is a semiconductor-metal heterojunction;
[0015] If the low-pressure phase is a metal, the high-pressure phase is still a metal, which is a metal-metal heterojunction.
[0016] The beneficial effects of the present invention are as follows:
[0017] The present invention provides a method for preparing a heterojunction using a controllable pressure gradient, which is a portable method for preparing a heterojunction. A diamond anvil cell press is used to generate a controllable pressure gradient, so that the two ends of the sample are respectively located in a low-pressure phase and a high-pressure phase, thereby realizing the rapid preparation of a heterostructure at room temperature. In the present invention, ruby powder is used to characterize the pressure distribution of different design structures, and the realization of the controllable pressure gradient is confirmed; further, suitable samples can be selected to prepare various types of heterojunction devices, which are suitable for the fields of rectifier devices and photoelectric detection. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.
[0019] Figure 1 A schematic diagram showing the process of preparing a heterojunction using a controllable pressure gradient in the present invention;
[0020] Figure 2 The pressure gradient distribution designed by the present invention is shown;
[0021] Figure 3 The test results of the heterostructure construction of CuFeS2 sample in Example 1 of the present invention are shown;
[0022] Figure 4 The IV characteristic test results of the heterostructure constructed for Si samples in Example 2 of the present invention are shown;
[0023] Figure 5 The photocurrent response test results of the heterostructure constructed for Si samples in Example 2 of the present invention are shown. DETAILED DESCRIPTION
[0024] In this embodiment, there is no special requirement for the size of the diamond anvil press, and different sizes of DACs such as 300, 400, and 500 μm anvil surfaces can be selected according to the pressure requirements. The present invention takes a 300 μm anvil surface DAC as an example. T301 stainless steel sheet is selected as the initial gasket material.
[0025] First, the gasket is pre-pressed to a thickness of ~40μm. Then, a laser drilling device is used to drill a hole with a radius of 140μm at the center of the indentation, and the gasket is cleaned and reset to the center of the DAC anvil surface. Boron nitride powder is filled in the hole and pre-pressed to a thickness of ~40μm for a second time. Figure 1 As shown in the left picture in the figure. At this time, the material of the gasket in contact with the diamond anvil surface is replaced by insulating boron nitride powder from stainless steel to provide insulation for the subsequent electrode placement. Then, the laser punching device is used again to cut out the specified shape (circular, square, etc.). Then, the gasket is reset to the center of the DAC anvil surface and fixed. Sodium chloride powder is filled in the specified shape area and compacted. At this point, the gasket preparation is completed, as shown in the figure below. Figure 1 As shown in the second picture from the left.
[0026] Before implementing the example, the invention confirmed the generation of controllable pressure gradient. Ruby powder was spread on the gasket after the preparation work was completed for pressure calibration. The pressure distribution of the diamond anvil surface when the center (NaCl area) pressure was 5GPa, 10GPa, 15GPa and 20GPa was plotted respectively, as shown in Figure 2. Figure 2 As shown. When the cutting shape is a square hole, there is an obvious difference in the pressure of different pressure-transmitting medium areas on both sides of the interface. When the central pressure is 5GPa, a pressure difference Δp=2~4GPa can be generated; when the central pressure is 10GPa, Δp=5~7GPa; when the central pressure is 15GPa, Δp=8~11GPa; when the central pressure is 20GPa, Δp=12~15GPa. And when the NaCl area deviates from the center, the range of the pressure gradient generated is larger, which is conducive to the operation of larger samples. Therefore, in the present invention, Figure 2 The subsequent heterojunction construction and characterization are carried out using the III method.
[0027] The sample can be selected from inorganic materials or organic-inorganic hybrid materials, etc., which need to undergo structural phase change under high pressure to meet the basic requirements of heterogeneous structure construction. The sample is cut into appropriate sizes in advance and placed in the center of the anvil surface so that one end is located in the NaCl area and the other end is located in the cBN area. Figure 1 As shown in the second picture from the middle right. Then, a ruby is placed near the sample in each area for pressure calibration. Gold or platinum wires are connected to both ends of the sample as lead wires for subsequent electrical measurements. Finally, pressure is applied to cause the cBN end sample to undergo a structural phase change to a high-pressure phase while the NaCl end sample remains in the initial low-pressure phase. At this point, the structures at both ends of the sample are different, and an interface is formed at the junction of the two pressure-transmitting media, thus realizing the preparation of a heterojunction in the pressure chamber, as shown in Figure 1. Figure 1 As shown in the middle right picture, the structure and performance of the prepared heterojunction can be further characterized.
[0028] Example 1
[0029] Preparation of heterojunction on CuFeS2 single crystal sample:
[0030] In order to verify the feasibility of the invention, some potential materials were selected for the preparation of heterojunctions.
[0031] In this case, a CuFeS2 single crystal sample is used as an example. According to existing research reports, CuFeS2 undergoes a structural phase transition near 8GPa accompanied by a change in carrier type from electrons to holes. In addition, it exhibits semiconductor behavior within 30GPa.
[0032] In this context, CuFeS2 is selected as the sample to prepare p-CuFeS2 / n-CuFeS2 pn-type semiconductor heterojunction. After the CuFeS2 sample is cut into a suitable size, it is placed in the center of the pretreated gasket, and the ruby and lead-out electrodes are placed and pressurized. The ruby calibration pressure at the NaCl end is 6.6GPa, and the ruby calibration pressure at the cBN end is 10.2GPa. At this time, the sample at the cBN part undergoes a phase change and the carrier type changes to holes, while the NaCl end is still the initial phase with electrons as the carrier type. Its electrical behavior (IV characteristic curve) is shown as follows Figure 3 As shown in the figure, there is an obvious rectification characteristic, which is one of the pn junction characteristics. This shows that the p-CuFeS2 / n-CuFeS2p-n semiconductor heterojunction was successfully prepared with the help of the pressure gradient generated by the diamond anvil, and the heterostructure has good rectification characteristics.
[0033] Example 2
[0034] Preparation of heterojunction on Si single crystal samples:
[0035] The experimental operation is the same as the above, and a Si single crystal sample is selected as an example in this example. According to existing research reports, Si will undergo a transition from a semiconductor phase (Si-I structure) to a metal phase (β-Sn structure) at around 10GPa. Based on this background, Si is selected as a sample to prepare an s-Si / m-Si semiconductor-metal heterojunction.
[0036] The test results after heterojunction preparation are as follows Figure 4 As shown, the IV characteristic curve exhibits nonlinear behavior and has certain rectification characteristics, indicating that the semiconductor-metal junction formed is a Schottky junction. In addition, the existence of photocurrent response under zero bias also proves the existence of a built-in electric field. It also shows that the s-Si / m-Si semiconductor-metal heterojunction was successfully prepared with the help of the pressure gradient generated by the diamond anvil cell. The heterostructure has certain rectification characteristics and good photocurrent response, which can be used in the field of self-powered optical detection.
[0037] The above examples prove the feasibility of the present invention. The portable preparation of heterojunctions using a diamond anvil cell with a controllable pressure gradient is universal in terms of materials, such as inorganic materials, organic-inorganic hybrid materials, etc. In addition, the design types of pressure gradients are also diverse, and different gasket types and shapes can be designed according to specific pressure requirements.
Claims
1. A method for preparing a heterojunction using a controllable pressure gradient, characterized in that: The process includes the following: by designing a controllable pressure gradient on the anvil surface of a diamond anvil device, the two ends of the sample are located in a low-pressure area and a high-pressure area respectively, and the pressure is applied to cause a phase change in the sample in the high-pressure area to achieve the construction of a heterojunction; The specific steps include: S1. Gasket preparation: Select T301 stainless steel sheet as the initial gasket material, pre-press the gasket to a thickness of ~40μm, then use a laser punching device to punch a hole with a radius of 140μm at the center of the indentation, clean the gasket and reset it to the center of the DAC anvil surface, fill the hole with boron nitride powder and pre-press it to a thickness of ~40μm for the second time; then use the laser punching device to cut out the specified shape again; then reset the gasket to the center of the DAC anvil surface and fix it; fill the specified shape area with sodium chloride powder and compact it; A regular shape is cut out of the boron nitride cBN region and filled with NaCl. Due to the difference in bulk modulus between cBN and NaCl during compression, a certain pressure gradient is formed between the two regions during compression. The pressure distribution on the diamond anvil surface was calibrated by ruby powder to confirm the formation of a controllable pressure gradient; S2. Select the sample; cut the sample into a suitable size and place it in the center of the anvil surface so that one end is located in the NaCl area and the other end is located in the cBN area. Then place a ruby in each area close to the sample for pressure calibration; and connect gold wires or platinum wires at both ends of the sample as lead wires for subsequent electrical measurements; S3. Pressurizing the device; Pressurizing causes the cBN-end sample to undergo a structural phase change to a high-pressure phase while the NaCl-end sample remains in the initial low-pressure phase. At this time, the structures at both ends of the sample are different, and an interface is formed at the junction of the two pressure-transmitting media, thereby realizing the preparation of a heterojunction in the pressure chamber.
2. A heterojunction, characterized in that: Obtained according to the method of claim 1.
3. A heterojunction according to claim 2, characterized in that: Depending on the different physical properties of the low-pressure phase and high-pressure phase of the selected sample, various types of heterojunctions can be achieved, including: If the low-voltage phase is an n / p-type semiconductor, the high-voltage phase is still an n / p-type semiconductor, which is a heterojunction of the same type of semiconductor; If the low-voltage phase is an n / p-type semiconductor and the high-voltage phase is a p / n-type semiconductor, it is an inversion semiconductor heterojunction, i.e., a pn junction; If the low-voltage phase is an n / p-type semiconductor and the high-voltage phase is a metal, it is a semiconductor-metal heterojunction; If the low-pressure phase is a metal, the high-pressure phase is still a metal, which is a metal-metal heterojunction.
Citation Information
Patent Citations
Superconducting materials and methods of making the same
CA3189728A1
Device and method for transferring two-dimensional layered semiconductor material to diamond anvil cell
CN105973678A
High-pressure experiment sample preparation and characterization integrated combination method
CN112414807A
Method for preparing two-dimensional heterojunction material with specific rotation angle
CN114225839A
Method for manufacturing nitride-based compound semiconductor substrate
JP2004307278A