A high-toughness ultra-thin glass and preparation method thereof

Through chemical thinning and secondary ion exchange treatment, high-tough ultra-thin glass, combined with carbon-fluorocarbon bond and ion exchange technology, the problem of glass brittleness and low bending strength is solved, and high-strength and anti-fouling performance is improved. It has self-healing function.

CN118439798BActive Publication Date: 2024-11-19SICHUAN SILICON BLUE NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410524713.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-28
Publication Date
2024-11-19
Estimated Expiration
2044-04-28

AI Technical Summary

Technical Problem

The brittleness and low bending strength of existing glasses limit their application in the field of electronic displays, and are difficult to meet the requirements of lightweight and high strength.

Method used

By chemically thinning and secondary ion exchange of glass and coating the surface with a surface treatment solution containing tetrafluoroethylene and 3-aminopropylene polymer, combined with mixed calcination of silica, aluminum hydroxide and sodium hydroxide Glass is obtained and ion exchange treatment is carried out in molten salts of ammonium fluoride, oxalic acid, ammonium sulfate, potassium nitrate and sodium nitrate to enhance the toughness and antifouling properties of the glass.

Benefits of technology

It significantly improves the bending strength and toughness of the glass, and has good anti-fouling ability. The surface coating can be self-healed under moisture stimulation.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high-toughness ultra-thin glass and a preparation method thereof, and relates to the field of glass. When preparing the high-toughness ultra-thin glass, the present invention polymerizes tetrafluoroethylene and 3-aminopropylene and then reacts with 2-formylphenylboric acid to obtain a surface treatment liquid; silicon dioxide, aluminum hydroxide and sodium hydroxide are mixed, calcined to obtain glass, and after washing, immersed in a mixed solution of ammonium fluoride, oxalic acid, ammonium sulfate and deionized water, and then immersed in potassium nitrate and sodium nitrate mixed molten salt and potassium nitrate molten salt in turn, and the surface is coated with the surface treatment liquid, dried, and the high-toughness ultra-thin glass is obtained. The high-toughness ultra-thin glass prepared by the present invention has anti-fouling ability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of glass, and in particular to high-toughness ultra-thin glass and a preparation method thereof. Background Art

[0002] Glass is a non-crystalline inorganic non-metallic material with good optical properties, mechanical properties and compressive strength. It is widely used in many fields such as architectural decoration, precision instruments, navigation and aerospace, electronic displays, new electric light sources, etc. However, the brittleness and low bending strength of glass limit its application range and actual performance.

[0003] With the progress of society, the emergence of electronic products and the ultra-large-scale application of the electronics industry have led to increasing requirements for the thinness and high strength of electronic display glass in actual use. How to achieve thinness and functionality while maintaining the strength of the glass is a problem that needs to be solved urgently. This article introduces a high-toughness ultra-thin glass with anti-fouling ability. Summary of the invention

[0004] The object of the present invention is to provide a high-toughness ultra-thin glass and a preparation method thereof, so as to solve the problems existing in the prior art.

[0005] The invention discloses a high-toughness ultra-thin glass, which is obtained by chemically thinning the glass and performing secondary ion exchange, coating the surface with a surface treatment liquid, and drying the glass.

[0006] As an optimization, the glass is obtained by mixing silicon dioxide, aluminum hydroxide and sodium hydroxide and calcining them.

[0007] As an optimization, the chemical thinning is to wash the glass and then immerse it in a mixture of ammonium fluoride, oxalic acid, ammonium sulfate and deionized water.

[0008] As an optimization, the secondary ion exchange is to immerse the glass in a mixed molten salt of potassium nitrate and sodium nitrate and a molten salt of potassium nitrate in sequence.

[0009] As an optimization, the surface coating surface treatment liquid is prepared by first polymerizing tetrafluoroethylene and 3-aminopropylene and then reacting with 2-formylphenylboronic acid.

[0010] A method for preparing high-toughness ultra-thin glass, the method for preparing high-toughness ultra-thin glass mainly comprises the following preparation steps:

[0011] (1) heating isopropanol to 140-144° C., adding an olefin mixture of 0.3-0.5 times the mass of isopropanol and azobisisobutyronitrile of 0.006-0.01 times the mass of isopropanol at a uniform rate over 4-6 hours, heating to 145-155° C., continuing the reaction for 100-140 minutes, cooling to 60-80° C., and adjusting the pH to 6.5-7.5 with dimethylisopropanolamine to obtain a polyolefin emulsion;

[0012] (2) Mixing the polyolefin emulsion with 2-formylphenylboronic acid in an equal molar amount of the amino group of the polyolefin emulsion, immersing in isopropanol, stirring at 200-300 r / min for 2.5-3.5 days, cooling to -2-2°C, adding sodium borohydride in an amount of 2-4 times the molar amount of the amino group of the polyolefin emulsion within 8-10 minutes, continuing stirring for 10-14 hours, drying at 60-70°C for 10-12 hours, washing with deionized water for 3-5 times, drying at 80-90°C for 8-10 hours, adding hexafluoroisopropanol in an amount of 0.5-0.7 times the mass of the olefin mixture, and preparing a surface treatment solution;

[0013] (3) keeping the crucible in a glass melting furnace at 1460-1500° C. for 10-20 min, taking it out, mixing silicon dioxide, aluminum hydroxide and sodium hydroxide in a molar ratio of 30-34:4-8:8-10 and adding them into the crucible, placing it in a glass melting furnace to react for 50-70 min, annealing it at 180-220° C. for 600-800 s, placing it in a mold, and casting it to obtain glass;

[0014] (4) After cleaning the glass, dry it at 50-60° C. for 22-24 hours; mix ammonium fluoride, oxalic acid, ammonium sulfate and deionized water in a mass ratio of 10-20:25-35:6-8:180-220, and perform ultrasonic treatment for 50-70 minutes to prepare a chemical etching solution; immerse the glass in the chemical etching solution until the glass thickness reaches 0.03-0.05 mm to prepare ultra-thin glass;

[0015] (5) The ultra-thin glass is placed in a preheating furnace, heated to 370-380°C at a heating rate of 8-12°C / min, and kept warm for 15-25 minutes. Then, it is immersed in a mixed molten salt of potassium nitrate and sodium nitrate in a molar ratio of 7:3, and ion exchange is performed at 380-400°C for 2-4 hours. After cooling to room temperature, it is placed in a mixed solution of deionized water and ethanol in a mass ratio of 1:1, and kept warm at 70-90°C for 15-25 minutes. Then, it is taken out and placed in a preheating furnace again at 8-12°C. The glass was heated to 370-380°C at a heating rate of 800-1200 r / min and kept warm for 15-25 min, immersed in potassium nitrate molten salt, subjected to secondary ion exchange at 380-400°C for 2-4 h, cooled to room temperature, put into a mixed solution of deionized water and ethanol in a mass ratio of 1:1, dried at 50-60°C for 6-8 h, spin-coated with the surface treatment liquid on the glass surface at 800-1200 r / min, and dried at 70-90°C for 50-70 min to obtain high-toughness ultra-thin glass.

[0016] As an optimization, the olefin mixture in step (1) is prepared by uniformly mixing tetrafluoroethylene and 3-aminopropylene in a molar ratio of 8-10:1-2.

[0017] As an optimization, the cleaning method of step (4) is to first clean with coconut amine for 3 to 5 times, then put it into a mixed solution of deionized water: ethanol in a mass ratio of 1:1 and ultrasonicate for 15 to 25 minutes, and dry it at 50 to 60°C for 22 to 24 hours.

[0018] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0019] When preparing high-toughness ultra-thin glass, the present invention polymerizes tetrafluoroethylene and 3-aminopropylene and then reacts with 2-formylphenylboric acid to obtain a surface treatment liquid; silicon dioxide, aluminum hydroxide and sodium hydroxide are mixed, calcined to obtain glass, and after washing, the glass is immersed in a mixed solution of ammonium fluoride, oxalic acid, ammonium sulfate and deionized water, and then immersed in a mixed molten salt of potassium nitrate and sodium nitrate and a molten salt of potassium nitrate in sequence, and the surface treatment liquid is coated on the surface, and the glass is dried to obtain high-toughness ultra-thin glass.

[0020] Firstly, when preparing high-toughness ultra-thin glass, the present invention polymerizes tetrafluoroethylene and 3-aminopropylene and then reacts with 2-formylphenylboronic acid to obtain a surface treatment liquid. The surface treatment liquid is rich in carbon-fluorine bonds, the carbon-fluorine bond covalent radius is small, and the fluorine atoms can shield the carbon chain well to maintain a high degree of stability. At the same time, due to the small polarizability and short bond distance of the carbon-fluorine bond, the intermolecular cohesion of the compound containing a large number of carbon-fluorine bonds is small, and the surface free energy is reduced, thereby achieving an anti-fouling effect; the nitrogen-coordinated boron oxygen hexacyclic ring in the surface treatment liquid is a reversible dynamic covalent force, which can be spontaneously opened under the stimulation of moisture, and the force is re-formed as the water molecules are lost, thereby achieving a self-repairing effect, so that the glass surface coating can be self-repaired by indoor water vapor at room temperature after being damaged.

[0021] Secondly, silicon dioxide, aluminum hydroxide and sodium hydroxide are mixed and calcined to obtain glass. After washing, the glass is immersed in a mixture of ammonium fluoride, oxalic acid, ammonium sulfate and deionized water, and then immersed in a mixed molten salt of potassium nitrate and sodium nitrate and a molten salt of potassium nitrate in turn. A surface treatment liquid is coated on the surface and dried to obtain high-toughness ultra-thin glass. The ion exchange method utilizes the ion exchange effect between glass and a large number of sodium ions or potassium ions to replace small ions with large ions such as sodium ions or potassium ions, thereby improving the strength of the glass and enhancing the toughness of the glass. In addition, this article adopts a secondary ion exchange method. The first ion exchange increases the depth of the ion exchange, and the second ion exchange increases the amount of ion exchange on the surface to obtain a larger surface compressive stress. Using the secondary ion exchange method, the stress layer is deeper than the primary ion exchange method, and the stress gradient inside the glass is further increased, thereby improving the surface hardness and bending strength of the glass and enhancing the toughness of the glass. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0023] Example 1

[0024] A high-toughness ultra-thin glass and a preparation method thereof, mainly comprising the following preparation steps:

[0025] (1) heating isopropanol to 140° C., adding an olefin mixture of 0.3 times the mass of isopropanol and azobisisobutyronitrile of 0.006 times the mass of isopropanol at a uniform rate over 4 hours, heating to 145° C., continuing the reaction for 100, cooling to 60° C., and adjusting the pH to 6.5 with dimethylisopropanolamine to obtain a polyolefin emulsion;

[0026] (2) The polyolefin emulsion and the polyolefin emulsion amino group were mixed with 2-formylphenylboronic acid in an equal molar amount, immersed in isopropanol, stirred at 200 r / min for 2.5 days, cooled to -2°C, and sodium borohydride in an amount twice the molar amount of the polyolefin emulsion amino group was added in 8, and the stirring was continued for 10 hours, and the mixture was dried at 60°C for 10 hours, washed with deionized water for 3 times, and dried at 80°C for 8 hours, and hexafluoroisopropanol in an amount of 0.5 times the mass of the polyolefin mixture was added to prepare a surface treatment solution;

[0027] (3) keeping the crucible in a glass melting furnace at 1460° C. for 10 min, taking it out, mixing silicon dioxide, aluminum hydroxide and sodium hydroxide in a molar ratio of 30:4:8 into the crucible, placing it in a glass melting furnace to react for 50 min, annealing at 180° C. for 600 s, placing it in a mold, and casting it to obtain glass;

[0028] (4) After cleaning the glass, dry it at 50° C. for 22 h; mix ammonium fluoride, oxalic acid, ammonium sulfate and deionized water in a mass ratio of 10:25:6:180, and perform ultrasonic treatment for 50 min to prepare a chemical etching solution; immerse the glass in the chemical etching solution until the glass thickness reaches 0.03 mm, thereby preparing ultra-thin glass;

[0029] (5) The ultra-thin glass was placed in a preheating furnace, heated to 370°C at a heating rate of 8°C / min and kept warm for 15 minutes, then immersed in a mixed molten salt of potassium nitrate and sodium nitrate in a molar ratio of 7:3, and subjected to a primary ion exchange at 380°C for 2 hours. After cooling to room temperature, the glass was placed in a mixed solution of deionized water and ethanol in a mass ratio of 1:1, kept warm at 70°C for 15 minutes, and then taken out. The glass was placed in a preheating furnace again, heated to 370°C at a heating rate of 8°C / min and kept warm for 15 minutes. The glass was immersed in a potassium nitrate molten salt, subjected to a secondary ion exchange at 380°C for 2 hours. After cooling to room temperature, the glass was placed in a mixed solution of deionized water and ethanol in a mass ratio of 1:1, and dried at 50°C for 6 hours. The surface treatment liquid was spin-coated on the glass surface at 800 r / min, and dried at 70°C for 50 minutes to obtain a high-toughness ultra-thin glass.

[0030] Example 2

[0031] A high-toughness ultra-thin glass and a preparation method thereof, mainly comprising the following preparation steps:

[0032] (1) heating isopropanol to 142° C., adding an olefin mixture of 0.4 times the mass of isopropanol and azobisisobutyronitrile of 0.008 times the mass of isopropanol at a uniform rate over 5 hours, heating to 150° C., continuing the reaction for 120 minutes, cooling to 70° C., and adjusting the pH to 7 with dimethylisopropanolamine to obtain a polyolefin emulsion;

[0033] (2) The polyolefin emulsion and the polyolefin emulsion amino group were mixed with 2-formylphenylboronic acid in an equal molar amount, immersed in isopropanol, stirred at 250 r / min for 3 days, cooled to 0°C, and sodium borohydride in an amount of 3 times the molar amount of the polyolefin emulsion amino group was added within 9 minutes, and the stirring was continued for 12 hours, and the mixture was dried at 65°C for 11 hours, washed with deionized water for 4 times, and dried at 85°C for 9 hours, and hexafluoroisopropanol in an amount of 0.6 times the mass of the olefin mixture was added to prepare a surface treatment solution;

[0034] (3) The crucible is kept in a glass melting furnace at 1480° C. for 15 min, taken out, silicon dioxide, aluminum hydroxide and sodium hydroxide are mixed in a molar ratio of 32:6:9 and added to the crucible, placed in a glass melting furnace for reaction for 60 min, annealed at 200° C. for 700 s, placed in a mold, and cast to obtain glass;

[0035] (4) After cleaning the glass, dry it at 55° C. for 23 h; mix ammonium fluoride, oxalic acid, ammonium sulfate and deionized water in a mass ratio of 15:30:7:200, and ultrasonically treat for 60 min to prepare a chemical etching solution; immerse the glass in the chemical etching solution until the glass thickness reaches 0.04 mm, thereby preparing ultra-thin glass;

[0036] (5) The ultra-thin glass was placed in a preheating furnace, heated to 375°C at a heating rate of 10°C / min and kept warm for 20 minutes, then immersed in a mixed molten salt of potassium nitrate and sodium nitrate in a molar ratio of 7:3, and subjected to a primary ion exchange at 390°C for 3 hours. After cooling to room temperature, the glass was placed in a mixed solution of deionized water and ethanol in a mass ratio of 1:1, kept warm at 80°C for 20 minutes, taken out, and placed in a preheating furnace again, heated to 375°C at a heating rate of 10°C / min and kept warm for 20 minutes. The glass was immersed in a potassium nitrate molten salt, subjected to a secondary ion exchange at 390°C for 3 hours. After cooling to room temperature, the glass was placed in a mixed solution of deionized water and ethanol in a mass ratio of 1:1, dried at 55°C for 7 hours, and the surface treatment liquid was spin-coated on the glass surface at 1000 r / min, and dried at 80°C for 60 minutes to obtain a high-toughness ultra-thin glass.

[0037] Example 3

[0038] A high-toughness ultra-thin glass and a preparation method thereof, mainly comprising the following preparation steps:

[0039] (1) heating isopropanol to 144° C., adding an olefin mixture of 0.5 times the mass of isopropanol and azobisisobutyronitrile of 0.01 times the mass of isopropanol at a uniform rate over 6 hours, heating to 155° C., continuing the reaction for 140 minutes, cooling to 80° C., and adjusting the pH to 7.5 with dimethylisopropanolamine to obtain a polyolefin emulsion;

[0040] (2) The polyolefin emulsion and the polyolefin emulsion amino group were mixed with 2-formylphenylboronic acid in an equal molar amount, immersed in isopropanol, stirred at 300 r / min for 3.5 days, cooled to 2°C, and sodium borohydride in an amount of 4 times the molar amount of the polyolefin emulsion amino group was added within 10 minutes, and the stirring was continued for 14 hours, dried at 70°C for 12 hours, washed with deionized water for 5 times, dried at 90°C for 10 hours, and hexafluoroisopropanol in an amount of 0.7 times the mass of the olefin mixture was added to prepare a surface treatment solution;

[0041] (3) The crucible is kept in a glass melting furnace at 1500° C. for 20 min, taken out, silicon dioxide, aluminum hydroxide and sodium hydroxide are mixed in a molar ratio of 34:8:10 and added to the crucible, placed in a glass melting furnace for reaction for 70 min, annealed at 220° C. for 800 s, placed in a mold, and cast to obtain glass;

[0042] (4) After cleaning the glass, dry it at 60° C. for 24 h; mix ammonium fluoride, oxalic acid, ammonium sulfate and deionized water in a mass ratio of 20:35:8:220, and perform ultrasonic treatment for 70 min to prepare a chemical etching solution; immerse the glass in the chemical etching solution until the glass thickness reaches 0.05 mm, thereby preparing ultra-thin glass;

[0043] (5) The ultra-thin glass was placed in a preheating furnace, heated to 380°C at a heating rate of 12°C / min and kept warm for 25 minutes, then immersed in a mixed molten salt of potassium nitrate and sodium nitrate in a molar ratio of 7:3, and subjected to a primary ion exchange at 400°C for 4 hours. After cooling to room temperature, the glass was placed in a mixed solution of deionized water and ethanol in a mass ratio of 1:1, kept warm at 90°C for 25 minutes, and then taken out. The glass was placed in a preheating furnace again, heated to 380°C at a heating rate of 12°C / min and kept warm for 25 minutes. The glass was immersed in a molten salt of potassium nitrate, and subjected to a secondary ion exchange at 400°C for 4 hours. After cooling to room temperature, the glass was placed in a mixed solution of deionized water and ethanol in a mass ratio of 1:1, and dried at 60°C for 8 hours. The surface treatment liquid was spin-coated on the glass surface at 1200 r / min, and dried at 90°C for 70 minutes to obtain a high-toughness ultra-thin glass.

[0044] Comparative Example 1

[0045] A high-toughness ultra-thin glass and a preparation method thereof, mainly comprising the following preparation steps:

[0046] (1) heating isopropanol to 142° C., adding an olefin mixture of 0.4 times the mass of isopropanol and azobisisobutyronitrile of 0.008 times the mass of isopropanol at a uniform rate over 5 hours, heating to 150° C., continuing the reaction for 120 minutes, cooling to 70° C., and adjusting the pH to 7 with dimethylisopropanolamine to obtain a polyolefin emulsion;

[0047] (2) The polyolefin emulsion and the polyolefin emulsion amino group were mixed with 2-formylphenylboronic acid in an equal molar amount, immersed in isopropanol, stirred at 250 r / min for 3 days, cooled to 0°C, and sodium borohydride in an amount of 3 times the molar amount of the polyolefin emulsion amino group was added within 9 minutes, and the stirring was continued for 12 hours, and the mixture was dried at 65°C for 11 hours, washed with deionized water for 4 times, and dried at 85°C for 9 hours, and hexafluoroisopropanol in an amount of 0.6 times the mass of the olefin mixture was added to prepare a surface treatment solution;

[0048] (3) The crucible is kept in a glass melting furnace at 1480° C. for 15 min, taken out, silicon dioxide, aluminum hydroxide and sodium hydroxide are mixed in a molar ratio of 32:6:9 and added to the crucible, placed in a glass melting furnace for reaction for 60 min, annealed at 200° C. for 700 s, placed in a mold, and cast to obtain glass;

[0049] (4) After cleaning the glass, dry it at 55° C. for 23 h; mix ammonium fluoride, oxalic acid, ammonium sulfate and deionized water in a mass ratio of 15:30:7:200, and ultrasonically treat for 60 min to prepare a chemical etching solution; immerse the glass in the chemical etching solution until the glass thickness reaches 0.04 mm, thereby preparing ultra-thin glass;

[0050] (5) The ultra-thin glass was placed in a preheating furnace, heated to 375°C at a heating rate of 10°C / min and kept warm for 20 min, then immersed in a mixed molten salt of potassium nitrate and sodium nitrate in a molar ratio of 7:3, and subjected to a primary ion exchange at 390°C for 3 h. After cooling to room temperature, the glass was placed in a mixed solution of deionized water and ethanol in a mass ratio of 1:1, and dried at 55°C for 7 h. The surface treatment liquid was spin-coated on the glass surface at 1000 r / min, and dried at 80°C for 60 min to obtain high-toughness ultra-thin glass.

[0051] Comparative Example 2

[0052] A high-toughness ultra-thin glass and a preparation method thereof, mainly comprising the following preparation steps:

[0053] (1) heating isopropanol to 142° C., adding an olefin mixture of 0.4 times the mass of isopropanol and azobisisobutyronitrile of 0.008 times the mass of isopropanol at a uniform rate over 5 hours, heating to 150° C., continuing the reaction for 120 minutes, cooling to 70° C., and adjusting the pH to 7 with dimethylisopropanolamine to obtain a polyolefin emulsion;

[0054] (2) The polyolefin emulsion and the polyolefin emulsion amino group were mixed with 2-formylphenylboronic acid in an equal molar amount, immersed in isopropanol, stirred at 250 r / min for 3 days, cooled to 0°C, and sodium borohydride in an amount of 3 times the molar amount of the polyolefin emulsion amino group was added within 9 minutes, and the stirring was continued for 12 hours, and the mixture was dried at 65°C for 11 hours, washed with deionized water for 4 times, and dried at 85°C for 9 hours, and hexafluoroisopropanol in an amount of 0.6 times the mass of the olefin mixture was added to prepare a surface treatment solution;

[0055] (3) The crucible is kept in a glass melting furnace at 1480° C. for 15 min, taken out, silicon dioxide, aluminum hydroxide and sodium hydroxide are mixed in a molar ratio of 32:6:9 and added to the crucible, placed in a glass melting furnace for reaction for 60 min, annealed at 200° C. for 700 s, placed in a mold, and cast to obtain glass;

[0056] (4) After cleaning the glass, dry it at 55° C. for 23 h; mix ammonium fluoride, oxalic acid, ammonium sulfate and deionized water in a mass ratio of 15:30:7:200, and ultrasonically treat for 60 min to prepare a chemical etching solution; immerse the glass in the chemical etching solution until the glass thickness reaches 0.04 mm, thereby preparing ultra-thin glass;

[0057] (5) The ultra-thin glass was placed in a mixed solution of deionized water and ethanol in a mass ratio of 1:1, dried at 55°C for 7 hours, the surface treatment liquid was spin-coated on the glass surface at 1000 r / min, and dried at 80°C for 60 minutes to obtain a high-toughness ultra-thin glass.

[0058] Comparative Example 3

[0059] A high-toughness ultra-thin glass and a preparation method thereof, mainly comprising the following preparation steps:

[0060] (1) heating isopropanol to 142° C., adding 3-aminopropylene (0.4 times the mass of isopropanol) and azobisisobutyronitrile (0.008 times the mass of isopropanol) at a uniform rate over 5 hours, heating to 150° C., continuing the reaction for 120 minutes, cooling to 70° C., and adjusting the pH to 7 with dimethylisopropanolamine to obtain a polyolefin emulsion;

[0061] (2) The polyolefin emulsion and the polyolefin emulsion amino group were mixed with 2-formylphenylboronic acid in an equal molar amount, immersed in isopropanol, stirred at 250 r / min for 3 days, cooled to 0°C, and sodium borohydride in an amount of 3 times the molar amount of the polyolefin emulsion amino group was added within 9 minutes, and the stirring was continued for 12 hours, and the mixture was dried at 65°C for 11 hours, washed with deionized water for 4 times, and dried at 85°C for 9 hours, and hexafluoroisopropanol in an amount of 0.6 times the mass of the olefin mixture was added to prepare a surface treatment solution;

[0062] (3) The crucible is kept in a glass melting furnace at 1480° C. for 15 min, taken out, silicon dioxide, aluminum hydroxide and sodium hydroxide are mixed in a molar ratio of 32:6:9 and added to the crucible, placed in a glass melting furnace for reaction for 60 min, annealed at 200° C. for 700 s, placed in a mold, and cast to obtain glass;

[0063] (4) After cleaning the glass, dry it at 55° C. for 23 h; mix ammonium fluoride, oxalic acid, ammonium sulfate and deionized water in a mass ratio of 15:30:7:200, and ultrasonically treat for 60 min to prepare a chemical etching solution; immerse the glass in the chemical etching solution until the glass thickness reaches 0.04 mm, thereby preparing ultra-thin glass;

[0064] (5) The ultra-thin glass was placed in a preheating furnace, heated to 375°C at a heating rate of 10°C / min and kept warm for 20 minutes, then immersed in a mixed molten salt of potassium nitrate and sodium nitrate in a molar ratio of 7:3, and subjected to a primary ion exchange at 390°C for 3 hours. After cooling to room temperature, the glass was placed in a mixed solution of deionized water and ethanol in a mass ratio of 1:1, kept warm at 80°C for 20 minutes, and then taken out. The glass was placed in a preheating furnace again, heated to 375°C at a heating rate of 10°C / min and kept warm for 20 minutes. The glass was immersed in a potassium nitrate molten salt, subjected to a secondary ion exchange at 390°C for 3 hours. After cooling to room temperature, the glass was placed in a mixed solution of deionized water and ethanol in a mass ratio of 1:1, and dried at 55°C for 7 hours. The surface treatment liquid was spin-coated on the glass surface at 1000 r / min, and dried at 80°C for 60 minutes to obtain a high-toughness ultra-thin glass.

[0065] Test Example 1

[0066] Toughness test

[0067] The three-point bending test was conducted using a universal material testing machine produced by Hangzhou Xingao Technology Co., Ltd. According to the GB / T232 national standard, the bending strength = (3 × the maximum load applied by the test bench when the sample breaks × the span of the sample bench) / (2 × the width of the sample to be tested × the thickness of the sample to be tested 2 ). The maximum load applied by the test bench when the sample breaks is 1N. The results are shown in Table 1.

[0068] Table 1

[0069] Bending Strength Example 1 925.3MPa Example 2 926.5MPa Example 3 925.9MPa Comparative Example 1 746.3MPa Comparative Example 2 483.8MPa Comparative Example 3 926.1MPa

[0070] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 1, it can be found that the high-toughness ultra-thin glass prepared by the present invention has higher toughness.

[0071] From the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 1 in Table 1, it can be found that the bending strength of Examples 1, 2, and 3 is greater than that of Comparative Example 1, which indicates that the first ion exchange in the secondary ion exchange method increases the depth of ion exchange, and the second ion exchange increases the amount of ion exchange on the surface, thereby obtaining a larger surface compressive stress. The stress layer is deeper than that of the primary ion exchange method, further increasing the stress gradient inside the glass, enhancing the toughness of the glass, and increasing the bending strength of the material.

[0072] From the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 2, it can be found that the bending strength of Examples 1, 2, 3 is greater than that of Comparative Example 2, which illustrates that the ion exchange method can utilize the ion exchange effect between glass and a large number of sodium ions or potassium ions to replace small ions with large ions such as sodium ions or potassium ions, thereby improving the strength of the glass, enhancing the toughness of the glass, and increasing the bending strength of the material.

[0073] Test Example 2

[0074] Antifouling test

[0075] Test method: The sample was cut into 50 cm × 5 cm strips, and after a 10 min droplet continuous rolling test (glycerol 45%) and a mud pouring test (mud 45 wt%), the water contact angle and the mud contact angle were tested. The results are shown in Table 2.

[0076] Table 2

[0077] Water contact angle Mud contact angle Example 1 158.9° 148.9° Example 2 159.8° 149.2° Example 3 159.3° 148.6° Comparative Example 1 159.1° 148.3° Comparative Example 2 158.4° 147.9° Comparative Example 3 88.2° 74.3°

[0078] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 2, it can be found that the high-toughness ultra-thin glass prepared by the present invention has good anti-fouling ability.

[0079] From the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 3 in Table 2, it can be found that the water contact angles and mud contact angles of Examples 1, 2, 3 are larger than those of Comparative Example 3, which shows that the covalent radius of the carbon-fluorine bond is small, and the fluorine atom can shield the carbon chain very well to maintain a high degree of stability. At the same time, due to the small polarizability and short bond distance of the carbon-fluorine bond, the intermolecular cohesion of compounds containing a large number of carbon-fluorine bonds is small, and the surface free energy is reduced, thereby achieving an anti-fouling effect and increasing the water contact angle and mud contact angle of the material surface.

[0080] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing high-toughness ultra-thin glass, It is characterized in that The preparation method of the high-toughness ultra-thin glass mainly includes the following preparation steps: (1) heating isopropanol to 140-144°C, uniformly adding an olefin mixture of 0.3-0.5 times the mass of isopropanol and azobisisobutyronitrile of 0.006-0.01 times the mass of isopropanol within 4-6 hours, heating to 145-155°C, continuing the reaction for 100-140 minutes, cooling to 60-80°C, and adjusting the pH to 6.5-7.5 with dimethylisopropanolamine to obtain a polyolefin emulsion; wherein the olefin mixture is prepared by uniformly mixing tetrafluoroethylene and 3-aminopropylene in a molar ratio of 8-10: 1-2; (2) mixing the polyolefin emulsion with an equimolar amount of 2-formylphenylboronic acid in the amino group of the polyolefin emulsion, immersing the mixture in isopropanol, and stirring at 200-300 r / min for 2.5-3.5 days. Cool down to -2~2℃, add sodium borohydride with 2~4 times the molar amount of amino group in polyolefin emulsion within 8~10min, continue stirring for 10~14h, dry at 60~70℃ for 10~12h, wash with deionized water 3~5 times, dry at 80~90℃ for 8~10h, add hexafluoroisopropanol with 0.5~0.7 times the mass of polyolefin mixture to obtain surface treatment liquid; (3) Keep the crucible in a glass melting furnace at 1460~1500℃ for 10~20min, take it out, mix silicon dioxide, aluminum hydroxide and sodium hydroxide in a molar ratio of 30~34: 4~8: 8~10 and add it to the crucible, put it into the glass melting furnace to react for 50~70min, anneal at 180~220℃ for 600~800s, place it in a mold, cast it into shape, and obtain glass; (4) After cleaning the glass, Dry at 50-60°C for 22-24h; Mix ammonium fluoride, oxalic acid, ammonium sulfate and deionized water in a mass ratio of 10-20: 25-35: 6-8: 180-220, and ultrasonically treat for 50-70min to prepare a chemical etching solution; Immerse the glass in the chemical etching solution until the glass thickness reaches 0.03-0.05mm, to obtain ultra-thin glass; (5) placing the ultra-thin glass in a preheating furnace, heating the temperature to 370-380℃ at a heating rate of 8-12℃ / min, keeping the temperature for 15-25min, then immersing it in a mixed molten salt of potassium nitrate and sodium nitrate in a molar ratio of 7:3, performing a primary ion exchange at 380-400℃ for 2-4h, cooling to room temperature, placing it in a mixed solution of deionized water: ethanol in a mass ratio of 1:1, keeping the temperature at 70-90℃ for 15-25min, then taking it out, placing it in a preheating furnace again, heating the temperature to 370-380℃ at a heating rate of 8-12℃ / min, keeping the temperature for 15-25min, immersing it in a molten salt of potassium nitrate, performing a secondary ion exchange at 380-400℃ for 2-4h, cooling to room temperature, placing it in a mixed solution of deionized water: ethanol in a mass ratio of 1:1, Dry at 50~60℃ for 6~8h, spin-coat the surface treatment liquid on the glass surface at 800~1200r / min, and dry at 70~90℃ for 50~70min to obtain high-toughness ultra-thin glass.

2. A method for preparing high-toughness ultra-thin glass according to claim 1, It is characterized in that The cleaning method of step (4) is to first clean with coconut amine for 3 to 5 times, then put it into a mixed solution of deionized water: ethanol with a mass ratio of 1:1 and ultrasonicate for 15 to 25 minutes, and dry it at 50 to 60°C for 22 to 24 hours.

3. A high-toughness ultra-thin glass, It is characterized in that The high-toughness ultra-thin glass is prepared according to the method for preparing high-toughness ultra-thin glass according to any one of claims 1 to 2.