A kind of acidic group-terminated polyether-modified organosilicon leveling agent and preparation method thereof
By using acidic group-terminated polyether-modified silicone leveling agents, combined with the design of dimethylsiloxane segments and polyether side chains, the problem of insufficient recoating adhesion in the existing technology has been solved, and high performance has been achieved. Taking both adhesion and leveling into consideration, production costs are reduced.
Patent Information
- Application Number
- CN202410903783.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-08
AI Technical Summary
Existing polyether-modified silicone leveling agents have deficiencies in recoat adhesion, making it difficult to balance both leveling and adhesion.
Polyether-modified silicone leveling agent capped with acidic groups is used. By introducing terminal acidic groups and combining the design of dimethylsiloxane segments and polyether side chains, the structure of the leveling agent is optimized to improve the film quality. Adhesion between layers.
While ensuring smoothness and leveling properties, it significantly improves recoating adhesion and reduces production costs. By controlling the composition of polyether side chains, leveling properties and adhesion are optimized.
Smart Images

Figure CN118440331B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of leveling agents, and particularly relates to an acid-group-terminated polyether-modified silicone leveling agent and a preparation method thereof. Background Art
[0002] Leveling agents are a type of functional additives widely used in industrial products such as coatings, inks, and resins. Their main function is to improve the fluidity of the coating film, thereby enhancing the surface quality and appearance of the coating. The introduction of leveling agents can significantly reduce defects such as shrinkage holes, fisheyes, and orange peel on the coating surface, making the coating more uniform and flat.
[0003] Silicone leveling agents refer to polydimethylsiloxane and its modified products, which have good substrate wetting and anti-shrinkage hole properties. Polyether-modified polysiloxanes are prepared by introducing polyether segments onto the polysiloxane main chain through block or grafting methods, which can significantly improve the compatibility of the products. However, such products have problems with poor recoat adhesion. Summary of the Invention
[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. For this purpose, the present invention provides an acid-group-terminated polyether-modified silicone leveling agent and a preparation method thereof. By introducing terminal acid group modification, while maintaining a high smoothness of the leveling agent, it also has good recoat performance.
[0005] According to the first aspect of the present invention, there is provided an acid-group-terminated polyether-modified silicone leveling agent having the following structural formula:
[0006] ;
[0007] wherein, m, n, p, and q are all integers, m = 2 - 10, n = 0 - 100, p = 5 - 50, q = 0 - 30, and it satisfies: when q = 0, n = 5 - 30; or when 0 < q ≤ 30, n = 5 - 20;
[0008] R is selected from H2PO3, COC2H4COOH, COC2H2COOH, or SO3H.
[0009] Preferably, in the above structural formula, n = 5 - 20, p = 30 - 50, q = 0 - 10.
[0010] Preferably, the molecular weight of the main chain of the acid-group-terminated polyether-modified silicone leveling agent is 500 - 3000; and / or, the molecular weight of the polyether side chain is 500 - 1000.
[0011] Preferably, the acid value of the leveling agent is 29 - 500 mgKOH / g.
[0012] More preferably, the acid value of the leveling agent is 30-60 mgKOH / g. The acid value of the modified organic silicon leveling agent of the present invention is controlled within this range, which can reduce production costs while ensuring excellent recoating adhesion.
[0013] It should be noted that the acidic group-terminated polyether-modified silicone leveling agent described in the present invention is not necessarily a block copolymer, and m, n, p, and q only represent the number of corresponding groups. The connection sequence of each group can be random or block, and the present invention does not impose any limitation on this.
[0014] According to a second aspect of the present invention, a method for preparing the acidic group-terminated polyether-modified silicone leveling agent as described in the first aspect of the present invention is provided, comprising the following steps:
[0015] S1: Hexamethyldisiloxane (MM), octamethylcyclotetrasiloxane (D4), tetramethylcyclotetrasiloxane (D4H) and the first catalyst are mixed and heated to react to obtain hydrogen-containing silicone oil;
[0016] S2: mixing the hydrogen-containing silicone oil, allyl polyether and the second catalyst, heating and reacting to obtain polyether-modified silicone oil;
[0017] S3: mixing the polyether-modified silicone oil and the acid anhydride, heating and reacting, and obtaining an acid group-terminated polyether-modified silicone leveling agent.
[0018] The reaction formula of step S1 is as follows:
[0019]
[0020] Preferably, in step S1, the molar ratio of hexamethyldisiloxane, octamethylcyclotetrasiloxane and tetramethylcyclotetrasiloxane is 1:(1.25-7.5):(0.5-1.5).
[0021] Preferably, in step S1, the first catalyst is selected from acidic clay.
[0022] Preferably, in step S1, the temperature of the heating reaction is 30-60° C., and the insulation time is 8-12 hours.
[0023] The reaction formula of step S2 is as follows:
[0024]
[0025] In the structural formula of the allyl polyether, R' is H or an epoxy group.
[0026] Preferably, R' is H.
[0027] Preferably, in step S2, the molar ratio of the hydrogen-containing silicone oil to the allyl polyether is 1:m.
[0028] Preferably, in step S2, the second catalyst is selected from a Castel catalyst.
[0029] Preferably, in step S2, the temperature of the heating reaction is 70-100° C., and the insulation time is 3-6 hours.
[0030] The reaction formula of step S3 may be as follows:
[0031]
[0032] or:
[0033]
[0034] or:
[0035]
[0036] or:
[0037]
[0038] Preferably, in step S3, the molar ratio of the polyether-modified silicone oil to the acid anhydride is 1:m.
[0039] Preferably, in step S3, the acid anhydride is at least one of maleic anhydride, succinic anhydride, chlorosulfonic acid or phosphorus pentoxide.
[0040] Preferably, in step S3, the temperature of the heating reaction is 80-120° C., and the insulation time is 4-10 hours.
[0041] According to the third aspect of the present invention, the use of the acidic group-terminated polyether-modified silicone leveling agent as described in the first aspect of the present invention in coatings is proposed.
[0042] Preferably, the coating is selected from polyurethane coating or amino baking varnish coating.
[0043] According to one embodiment of the present invention, there are at least the following beneficial effects:
[0044] The modified organic silicon leveling agent of the present invention has a polyether side chain terminated by an acidic group, and the acidic group forms a strong hydrogen bond with the polar group in the coating film layer, thereby improving the adhesion between the film layers. At the same time, by controlling the content of the dimethylsiloxane segment and the siloxane segment with a polyether side chain, the leveling property and the adhesion can be taken into account. In the polyether side chain, appropriately increasing the content of the ethoxy group or appropriately reducing the content of the isopropoxy group is conducive to improving the adhesion. DETAILED DESCRIPTION
[0045] The concept and technical effects of the present invention will be clearly and completely described below in conjunction with embodiments to fully understand the purpose, features and effects of the present invention.
[0046] Unless otherwise specified, the raw materials, reagents or devices used in the following examples and comparative examples can be obtained from conventional commercial channels or by existing known methods, wherein the acidic clay was purchased from Qiangdong Mineral Products Processing Plant.
[0047] Example 1
[0048] This embodiment provides an acidic group-terminated polyether-modified organic silicon leveling agent, the structural formula of which is as follows:
[0049] .
[0050] The preparation process of the above-mentioned acidic group-terminated polyether-modified organic silicon leveling agent comprises the following steps:
[0051] (1) Add 162 g of hexamethyldisiloxane, 370 g of octamethylcyclotetrasiloxane and 120 g of tetramethylcyclotetrasiloxane into a four-necked flask, add 50 g of acid clay, stir evenly, heat to 50 °C and react for 10 h, and filter to obtain hydrogenated silicone oil (m=2, n=5) with a molecular weight of 652.
[0052] (2) 163 g of hydrogenated silicone oil, 284 g of allyl polyether HMS-229R (p=5, q=5, R' is H, purchased from Zhejiang Real Madrid) with a molecular weight of 568, and 0.4 g of Castel catalyst were added into a four-necked flask, stirred evenly, and kept warm at 80 °C for 4 h to obtain polyether modified silicone oil with a molecular weight of 1788.
[0053] (3) Add 178.8 g of polyether-modified silicone oil and 19.6 g of maleic anhydride (R is COC2H2COOH) into a four-necked flask and stir evenly. Heat to 80 °C and react for 4 h to obtain a product with an acid value of 56 mgKOH / g.
[0054] Example 2
[0055] This embodiment provides an acidic group-terminated polyether-modified organosilicon leveling agent, the structural formula of which is the same as that of Embodiment 1, and the synthesis method thereof comprises the following steps:
[0056] (1) Add 162 g of hexamethyldisiloxane, 592 g of octamethylcyclotetrasiloxane and 120 g of tetramethylcyclotetrasiloxane into a four-necked flask, add 50 g of acid clay, stir evenly, heat to 50 °C and react for 10 h, and filter to obtain hydrogenated silicone oil (m=2, n=8) with a molecular weight of 874.
[0057] (2) 87.4 g of hydrogenated silicone oil, 144 g of allyl polyether F5 (p=10.5, q=3.5, R' is H, purchased from Yangzhou Chenhua) with a molecular weight of 720, and 0.3 g of Castel catalyst were added into a four-necked flask, stirred evenly, and kept warm at 80°C for 4 h to obtain polyether-modified silicone oil with a molecular weight of 2314.
[0058] (3) Add 92.56 g of polyether-modified silicone oil and 7.84 g of maleic anhydride (R is COC2H2COOH) into a four-necked flask and stir evenly. Heat to 80 °C and react for 4 h to obtain a product with an acid value of 44 mgKOH / g.
[0059] Example 3
[0060] This embodiment provides an acidic group-terminated polyether-modified organosilicon leveling agent, the structural formula of which is the same as that of Embodiment 1, and the synthesis method thereof comprises the following steps:
[0061] (1) Add 162 g of hexamethyldisiloxane, 1110 g of octamethylcyclotetrasiloxane and 180 g of tetramethylcyclotetrasiloxane into a four-necked flask, add 50 g of acid clay, stir evenly, heat to 50 °C and react for 10 h, and filter to obtain hydrogenated silicone oil (m=3, n=15) with a molecular weight of 1452.
[0062] (2) 145.2 g of hydrogenated silicone oil, 302.4 g of allyl polyether AFEP-12 (p=15, q=5, R' is H, purchased from Zhongshan Chemical) with a molecular weight of 1008, and 0.6 g of Castel catalyst were added into a four-necked flask, stirred evenly, and kept warm at 80°C for 4 h to obtain polyether-modified silicone oil with a molecular weight of 4476.
[0063] (3) Add 44.76 g of polyether-modified silicone oil and 3 g of succinic anhydride (R is COC2H4COOH) into a four-necked flask and stir evenly. Heat to 80 °C and react for 4 h to obtain a product with an acid value of 35 mgKOH / g.
[0064] Example 4
[0065] This embodiment provides an acidic group-terminated polyether-modified organosilicon leveling agent, the structural formula of which is the same as that of Embodiment 1, and the synthesis method thereof comprises the following steps:
[0066] (1) Add 162 g of hexamethyldisiloxane, 1480 g of octamethylcyclotetrasiloxane and 240 g of tetramethylcyclotetrasiloxane into a four-necked flask, add 150 g of acid clay, stir evenly, heat to 50 °C and react for 10 h, and filter to obtain hydrogenated silicone oil (m=4, n=20) with a molecular weight of 1882.
[0067] (2) 188.2 g of hydrogenated silicone oil, 500 g of allyl polyether HMS-519R (p=17.5, q=7.5, R' is H, purchased from Zhejiang Real Madrid) with a molecular weight of 1250, and 0.6 g of Castel catalyst were added into a four-necked flask, stirred evenly, and kept warm at 80 °C for 4 h to obtain polyether modified silicone oil with a molecular weight of 6882.
[0068] (3) Add 68.82 g of polyether-modified silicone oil and 4.66 g of chlorosulfonic acid (R is SO3H) into a four-necked flask and stir evenly. Heat to 80 °C and react for 4 h to obtain a product with an acid value of 32 mgKOH / g.
[0069] Example 5
[0070] This embodiment provides an acidic group-terminated polyether-modified organosilicon leveling agent, the structural formula of which is the same as that of Embodiment 1, and the synthesis method thereof comprises the following steps:
[0071] (1) Add 162 g of hexamethyldisiloxane, 2220 g of octamethylcyclotetrasiloxane and 240 g of tetramethylcyclotetrasiloxane into a four-necked flask, add 150 g of acid clay, stir evenly, heat to 50 °C and react for 10 h, and filter to obtain hydrogenated silicone oil (m=4, n=30) with a molecular weight of 2622.
[0072] (2) Add 262.2 g of hydrogenated silicone oil, 607.2 g of allyl polyether SZA-1500 (p=33, q=0, R' is H, purchased from Shangzheng New Materials) with a molecular weight of 1510, and 0.5 g of Castel catalyst into a four-necked flask, stir evenly, and keep warm at 80°C for 4 h to obtain polyether modified silicone oil with a molecular weight of 8694.
[0073] (3) 86.94 g of polyether-modified silicone oil and 2.84 g of phosphorus pentoxide (R is H2PO3) were added into a four-necked flask and stirred evenly. The temperature was raised to 80°C and reacted for 4 h to obtain a product with an acid value of 49 mgKOH / g.
[0074] Comparative Example 1
[0075] This comparative example provides a polyether-modified silicone oil, the preparation process of which is different from that of Example 1 in that step (3) is not performed. Specifically, the following steps are included:
[0076] (1) Add 162 g of hexamethyldisiloxane, 370 g of octamethylcyclotetrasiloxane and 120 g of tetramethylcyclotetrasiloxane into a four-necked flask, add 50 g of acid clay, stir evenly, heat to 50 °C and react for 10 h, and filter to obtain hydrogenated silicone oil (m=2, n=5) with a molecular weight of 652.
[0077] (2) 163 g of hydrogenated silicone oil, 284 g of allyl polyether HMS-229R (p=5, q=5, R' is H, purchased from Zhejiang Real Madrid) with a molecular weight of 568, and 0.4 g of Castel catalyst were added into a four-necked flask, stirred evenly, and kept warm at 80 °C for 4 h to obtain polyether modified silicone oil with a molecular weight of 1788.
[0078] Comparative Example 2
[0079] This comparative example provides a polyether-modified silicone oil, the preparation process of which is different from that of Example 2 in that step (3) is not performed. Specifically, the following steps are included:
[0080] (1) Add 162 g of hexamethyldisiloxane, 592 g of octamethylcyclotetrasiloxane and 120 g of tetramethylcyclotetrasiloxane into a four-necked flask, add 50 g of acid clay, stir evenly, heat to 50 °C and react for 10 h, and filter to obtain hydrogenated silicone oil (m=2, n=8) with a molecular weight of 874.
[0081] (2) 87.4 g of hydrogenated silicone oil, 144 g of allyl polyether F5 (p=10.5, q=3.5, R' is H, purchased from Yangzhou Chenhua) with a molecular weight of 720, and 0.3 g of Castel catalyst were added into a four-necked flask, stirred evenly, and kept warm at 80°C for 4 h to obtain polyether-modified silicone oil with a molecular weight of 2314.
[0082] Comparative Example 3
[0083] This comparative example provides a polyether-modified silicone oil, the preparation process of which is different from that of Example 3 in that step (3) is not performed. Specifically, the following steps are included:
[0084] (1) Add 162 g of hexamethyldisiloxane, 1110 g of octamethylcyclotetrasiloxane and 180 g of tetramethylcyclotetrasiloxane into a four-necked flask, add 50 g of acid clay, stir evenly, heat to 50 °C and react for 10 h, and filter to obtain hydrogenated silicone oil (m=3, n=15) with a molecular weight of 1452.
[0085] (2) 145.2 g of hydrogenated silicone oil, 302.4 g of allyl polyether AFEP-12 (p=15, q=5, R' is H, purchased from Zhongshan Chemical) with a molecular weight of 1008, and 0.6 g of Castel catalyst were added into a four-necked flask, stirred evenly, and kept warm at 80°C for 4 h to obtain polyether-modified silicone oil with a molecular weight of 4476.
[0086] Comparative Example 4
[0087] This comparative example provides a polyether-modified silicone oil, which specifically comprises the following steps:
[0088] (1) Add 162 g of hexamethyldisiloxane, 2220 g of octamethylcyclotetrasiloxane and 240 g of tetramethylcyclotetrasiloxane into a four-necked flask, add 150 g of acid clay, stir evenly, heat to 50 °C and react for 10 h, and filter to obtain hydrogenated silicone oil (m=4, n=30) with a molecular weight of 2622.
[0089] (2) Add 262.2 g of hydrogenated silicone oil, 607.2 g of allyl polyether F-6-3 (p=20, q=10, R' is H, Zhongshan Chemical) with a molecular weight of 1518, and 2 g of Castel catalyst into a four-necked flask, stir evenly, and keep warm at 80°C for 4 h to obtain polyether-modified silicone oil with a molecular weight of 8694.
[0090] Comparative Example 5
[0091] This comparative example provides an acidic group-terminated polyether-modified organic silicon leveling agent, the structural formula of which is the same as that of Example 1, and the synthesis method thereof comprises the following steps:
[0092] (1) Add 162 g of hexamethyldisiloxane, 2220 g of octamethylcyclotetrasiloxane and 240 g of tetramethylcyclotetrasiloxane into a four-necked flask, add 150 g of acid clay, stir evenly, heat to 50 °C and react for 10 h, and filter to obtain hydrogenated silicone oil (m=4, n=30) with a molecular weight of 2622.
[0093] (2) Add 262.2 g of hydrogenated silicone oil, 607.2 g of allyl polyether F-6-3 (p=20, q=10, R' is H, Zhongshan Chemical) with a molecular weight of 1518, and 0.5 g of Custer catalyst into a four-necked flask, stir evenly, and keep warm at 80°C for 4 h to obtain polyether-modified silicone oil with a molecular weight of 8694.
[0094] (3) 86.94 g of polyether-modified silicone oil and 2.84 g of phosphorus pentoxide (R is H2PO3) were added into a four-necked flask and stirred evenly. The temperature was raised to 80°C and reacted for 4 h to obtain a product with an acid value of 49 mgKOH / g.
[0095] Comparative Example 6
[0096] This comparative example provides an acidic group-terminated polyether-modified organic silicon leveling agent, the structural formula of which is the same as that of Example 1, and the synthesis method thereof comprises the following steps:
[0097] (1) Add 162 g of hexamethyldisiloxane, 2220 g of octamethylcyclotetrasiloxane and 240 g of tetramethylcyclotetrasiloxane into a four-necked flask, add 150 g of acid clay, stir evenly, heat to 50 °C and react for 10 h, and filter to obtain hydrogenated silicone oil (m=4, n=30) with a molecular weight of 2622.
[0098] (2) Add 262.2 g of hydrogenated silicone oil, 500 g of allyl polyether HMS-519R (p=17.5, q=7.5, R' is H, purchased from Zhejiang Real Madrid) with a molecular weight of 1250, and 0.6 g of Castel catalyst into a four-necked flask, stir evenly, and keep warm at 80°C for 4 h to obtain polyether modified silicone oil with a molecular weight of 7622.
[0099] (3) Add 76.22 g of polyether-modified silicone oil and 4.66 g of chlorosulfonic acid (R is SO3H) into a four-necked flask and stir evenly. Heat to 80 °C and react for 4 h to obtain a product with an acid value of 29 mgKOH / g.
[0100] Comparative Example 7
[0101] This comparative example provides an acidic group-terminated polyether-modified organic silicon leveling agent, the structural formula of which is the same as that of Example 1, and the synthesis method thereof comprises the following steps:
[0102] (1) Add 162 g of hexamethyldisiloxane, 2220 g of octamethylcyclotetrasiloxane and 240 g of tetramethylcyclotetrasiloxane into a four-necked flask, add 150 g of acid clay, stir evenly, heat to 50 °C and react for 10 h, and filter to obtain hydrogenated silicone oil (m=4, n=30) with a molecular weight of 2622.
[0103] (2) Add 262.2 g of hydrogenated silicone oil, 607.2 g of allyl polyether SZF-1500 (p=0, q=25, R' is H, purchased from Shangzheng New Materials) with a molecular weight of 1510, and 0.5 g of Castel catalyst into a four-necked flask, stir evenly, and keep warm at 80°C for 4 h to obtain polyether modified silicone oil with a molecular weight of 8694.
[0104] (3) 86.94 g of polyether-modified silicone oil and 2.84 g of phosphorus pentoxide (R is H2PO3) were added into a four-necked flask and stirred evenly. The temperature was raised to 80°C and reacted for 4 h to obtain a product with an acid value of 49 mgKOH / g.
[0105] Comparative Example 8
[0106] This comparative example provides a partially acidic group-terminated polyether-modified organic silicone leveling agent. The preparation process thereof is different from that of Example 1 in that the amount of acid anhydride in step (3) is changed. Specifically, the preparation process comprises the following steps:
[0107] (1) Add 162 g of hexamethyldisiloxane, 370 g of octamethylcyclotetrasiloxane and 120 g of tetramethylcyclotetrasiloxane into a four-necked flask, add 50 g of acid clay, stir evenly, heat to 50 °C and react for 10 h, and filter to obtain hydrogenated silicone oil (m=2, n=5) with a molecular weight of 652.
[0108] (2) 163 g of hydrogenated silicone oil, 284 g of allyl polyether HMS-229R (p=5, q=5, R' is H, purchased from Zhejiang Real Madrid) with a molecular weight of 568, and 0.4 g of Castel catalyst were added into a four-necked flask, stirred evenly, and kept warm at 80 °C for 4 h to obtain polyether modified silicone oil with a molecular weight of 1788.
[0109] (3) Add 178.8 g of polyether-modified silicone oil and 9.8 g of maleic anhydride (half of R is H and half of R is COC2H2COOH) into a four-necked flask and stir evenly. Heat to 80 °C and react for 4 h to obtain a product with an acid value of 28 mgKOH / g.
[0110] Comparative Example 9
[0111] This comparative example provides a partially acidic group-terminated polyether-modified organic silicon leveling agent. The preparation process thereof is different from that of Example 2 in that the amount of acid anhydride in step (3) is changed. Specifically, the preparation process comprises the following steps:
[0112] (1) Add 162 g of hexamethyldisiloxane, 592 g of octamethylcyclotetrasiloxane and 120 g of tetramethylcyclotetrasiloxane into a four-necked flask, add 50 g of acid clay, stir evenly, heat to 50 °C and react for 10 h, and filter to obtain hydrogenated silicone oil (m=2, n=8) with a molecular weight of 874.
[0113] (2) 87.4 g of hydrogenated silicone oil, 144 g of allyl polyether F5 (p=10.5, q=3.5, R' is H, purchased from Yangzhou Chenhua) with a molecular weight of 720, and 0.3 g of Castel catalyst were added into a four-necked flask, stirred evenly, and kept warm at 80°C for 4 h to obtain polyether-modified silicone oil with a molecular weight of 2314.
[0114] (3) Add 92.56 g of polyether-modified silicone oil and 3.92 g of maleic anhydride (half of R is H and half of R is COC2H2COOH) into a four-necked flask and stir evenly. Heat to 80 °C and react for 4 h to obtain a product with an acid value of 22 mgKOH / g.
[0115] Comparative Example 10
[0116] This comparative example provides a partially acidic group-terminated polyether-modified organic silicon leveling agent. The preparation process thereof is different from that of Example 3 in that the amount of acid anhydride in step (3) is changed. Specifically, the preparation process comprises the following steps:
[0117] (1) Add 162 g of hexamethyldisiloxane, 1110 g of octamethylcyclotetrasiloxane and 180 g of tetramethylcyclotetrasiloxane into a four-necked flask, add 50 g of acid clay, stir evenly, heat to 50 °C and react for 10 h, and filter to obtain hydrogenated silicone oil (m=3, n=15) with a molecular weight of 1452.
[0118] (2) 145.2 g of hydrogenated silicone oil, 302.4 g of allyl polyether AFEP-12 (p=15, q=5, R' is H, purchased from Zhongshan Chemical) with a molecular weight of 1008, and 0.6 g of Castel catalyst were added into a four-necked flask, stirred evenly, and kept warm at 80°C for 4 h to obtain polyether-modified silicone oil with a molecular weight of 4476.
[0119] (3) Add 44.76 g of polyether-modified silicone oil and 1 g of succinic anhydride (two-thirds of R is H and one-third of R is COC2H4COOH) into a four-necked flask and stir evenly. Heat to 80 °C and react for 4 h to obtain a product with an acid value of 12 mgKOH / g.
[0120] Comparative Example 11
[0121] This comparative example provides a partially acidic group-terminated polyether-modified silicone leveling agent, which specifically comprises the following steps:
[0122] (1) Add 162 g of hexamethyldisiloxane, 2220 g of octamethylcyclotetrasiloxane and 240 g of tetramethylcyclotetrasiloxane into a four-necked flask, add 150 g of acid clay, stir evenly, heat to 50 °C and react for 10 h, and filter to obtain hydrogenated silicone oil (m=4, n=30) with a molecular weight of 2622.
[0123] (2) Add 262.2 g of hydrogenated silicone oil, 607.2 g of allyl polyether F-6-3 (p=20, q=10, R' is H, purchased from Zhongshan Chemical) with a molecular weight of 1518, and 2 g of Castel catalyst into a four-necked flask, stir evenly, and keep warm at 80°C for 4 h to obtain polyether-modified silicone oil with a molecular weight of 8694.
[0124] (3) 86.94 g of polyether-modified silicone oil and 1.42 g of phosphorus pentoxide (half of R is H and half of R is H2PO3) were added into a four-necked flask and stirred evenly. The temperature was raised to 80°C and reacted for 4 h to obtain a product with an acid value of 25 mgKOH / g.
[0125] Test example
[0126] The products obtained in Examples 1 to 5 and Comparative Examples 1 to 11 were respectively used to prepare PU varnish, wherein the PU varnish was prepared by mixing component A and component B in a ratio of 100:40 by mass, and the compositions of the components A and B are shown in Table 1 below. The PU varnish was sprayed on the base plate, the film thickness was controlled to be 30 μm, and it was dried at 80°C for 1 hour. The same varnish was sprayed on the paint film for the second time, the film thickness was controlled to be 30 μm, and it was dried at 80°C for 1 hour. The recoating adhesion of the paint film was tested according to GB / T 9286-1998, and the friction coefficient of the paint film was tested according to GB / T10006-2021, and the results are shown in Table 2 below.
[0127]
[0128]
[0129] It can be seen that the larger the molecular weight of the silicone oil in the silicone leveling agent in the coating, the lower the friction coefficient of the formed paint film and the smoother the feel of the paint film. At the same time, it can be seen that for polyether-modified silicone leveling agents that are not terminated by acidic groups, the larger the molecular weight of the silicone oil, the worse the recoating performance. The polyether-modified silicone leveling agent completely terminated by acidic groups can significantly improve the recoating adhesion of the paint film, which is conducive to recoating construction while retaining its smoothness. The polyether-modified silicone leveling agent partially terminated by acidic groups can slightly improve the recoating adhesion of the paint film.
[0130] In the comparative examples without acidic group end-capping, the larger the molecular weight of the silicone oil, the stronger its ability to reduce surface tension, and thus the worse its recoating adhesion.
[0131] The recoating adhesion of Example 4 is better than that of Comparative Example 5 and Comparative Example 6, indicating that when the polyether side chain contains isopropoxy, appropriately reducing the content of dimethylsiloxane segments is beneficial to improving adhesion. From the performance comparison of Example 5, Comparative Example 5, and Comparative Example 7, it can be seen that reducing the content of isopropoxy in the polyether side chain and appropriately increasing the content of ethoxy is beneficial to improving recoating adhesion.
[0132] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
Claims
1. An organosilicon leveling agent, characterized in that: Has the following structural formula: Wherein, m, n, p, q are all integers, m = 2 ~ 10, n = 5 ~ 30, p = 5 ~ 33, q = 0 ~ 10, and satisfy: when q = 0, n = 5 ~ 30; or when 0 < q ≤ 10, n = 5 ~ 20; R is selected from H2PO3, COC2H4COOH, COC2H2COOH or SO3H; The acid value of the leveling agent is 32-60 mgKOH / g.
2. A method for preparing the organosilicon leveling agent according to claim 1, characterized in that: The following steps are involved: S1: mixing hexamethyldisiloxane, octamethylcyclotetrasiloxane, tetramethylcyclotetrasiloxane and a first catalyst, heating and reacting to obtain hydrogen-containing silicone oil; S2: mixing the hydrogen-containing silicone oil, allyl polyether and the second catalyst, heating and reacting to obtain polyether-modified silicone oil; S3: mixing the polyether-modified silicone oil with an acid anhydride, heating and reacting the mixture to obtain an organic silicone leveling agent; the acid anhydride is phosphorus pentoxide, succinic anhydride or maleic anhydride.
3. The preparation method according to claim 2, characterized in that: In step S1, the molar ratio of hexamethyldisiloxane, octamethylcyclotetrasiloxane and tetramethylcyclotetrasiloxane is 1:(1.25-7.5):(0.5-1.5).
4. The preparation method according to claim 2, characterized in that: In step S2, the molar ratio of the hydrogen-containing silicone oil to the allyl polyether is 1:m.
5. The preparation method according to claim 2, characterized in that: In step S3, the molar ratio of the polyether-modified silicone oil to the acid anhydride is 1:m.
6. The preparation method according to claim 2, characterized in that: In step S3, the temperature of the heating reaction is 80-120° C., and the insulation time is 4-10 hours.
7. Use of the organosilicon leveling agent according to claim 1 in coatings.