A composite material with low water absorption and water ripple appearance and preparation method thereof

Through the combination of raw materials such as modified carbon fiber, graphene oxide polymer and twin screw extrusion process, low water absorption rate water corrugated composite materials are prepared, which solves the problems of high water absorption rate and poor mechanical properties, and achieves excellent mechanical properties and better Broad market application.

CN118440488BActive Publication Date: 2024-11-08LIANYUNGANG SHENYING CARBON BIKE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410605353.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-16
Publication Date
2024-11-08
Estimated Expiration
2044-05-16

AI Technical Summary

Technical Problem

The existing water corrugated composite materials have problems of high water absorption and poor mechanical properties, which affects their application in military industry, aerospace and other fields.

Method used

Using modified carbon fiber, graphene oxide polymer, lubricant and antioxidant raw materials, low-water absorption water corrugated appearance composite materials are prepared through ultrasonic dispersion and twin-screw extruder granulation process to improve its tensile strength and bending strength .

Benefits of technology

It significantly reduces the water absorption rate of composite materials and increases its tensile strength and bending strength, suitable for a wider market, especially in areas with high performance requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118440488B_ABST
    Figure CN118440488B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of composite material production, in particular to a composite material with low water absorption and water ripple appearance and a preparation method thereof; the composite material is made of the following raw materials in parts by weight: 20 to 30 parts of modified carbon fiber, 8 to 12 parts of graphene oxide polymer, 10 to 20 parts of lubricant and 6 to 10 parts of antioxidant; the composite material prepared by the invention uses modified carbon fiber, graphene oxide polymer, lubricant and antioxidant as raw materials, and is weighed, and then the modified carbon fiber, graphene oxide polymer, lubricant and antioxidant are transferred into a mixing device for mixing, and finally placed in a twin-screw extruder for extrusion and granulation to obtain a composite material finished product; the prepared composite material not only has an excellent low water absorption effect, but also has excellent tensile strength and bending strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite material production, in particular to a composite material with a low water absorption rate and a water-ripple appearance and a preparation method thereof. Background Art

[0002] As a high-performance structural material, carbon fiber composite materials are widely used in military, aerospace and other fields because they have the characteristics of strong structural designability, simple process and obvious weight reduction effect when used to make structural parts.

[0003] Water-ripple products are popular in the market for their fashionable and personalized style that aligns with market trends. However, current water-ripple materials suffer from issues such as high water absorption and poor mechanical properties. Therefore, effectively improving the quality of composite materials with water-ripple appearance has become a critical issue that needs to be addressed in my country's composite materials manufacturing industry.

[0004] Therefore, the present invention provides a composite material with a low water absorption rate and a water-ripple appearance and a preparation method thereof, which are used to solve the above-mentioned related technical problems. Summary of the Invention

[0005] The purpose of the present invention is to provide a low water absorption water corrugated appearance composite material and a preparation method thereof. The composite material prepared by the present invention not only has excellent low water absorption effect; but also has excellent tensile strength and bending strength.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The first aspect of the present invention provides a low water absorption water corrugated appearance composite material, which is made of the following raw materials in parts by weight: 20 to 30 parts of modified carbon fiber, 8 to 12 parts of graphene oxide polymer, 10 to 20 parts of lubricant and 6 to 10 parts of antioxidant.

[0008] The present invention is further configured as follows: the preparation process of the modified carbon fiber is as follows:

[0009] The short carbon fibers were ultrasonically dispersed in an appropriate amount of acetone at a solid-liquid ratio of 0.02 to 0.05 g / mL for 20 to 30 minutes. After the ultrasonic dispersion was completed, the resulting dispersion was treated in a water bath at 60 to 68°C for 300 to 340 minutes, filtered, washed with deionized water for 4 to 6 times, and then dried at 70 to 72°C. Dry 50 ~60min, the carbon fiber is expected to be obtained;

[0010] The carbon fiber is ultrasonically dispersed in an appropriate amount of silane solution at a solid-liquid ratio of 0.05 to 0.07 g / mL for 30 to 40 minutes, and then heat-treated at a temperature of 78 to 82° C. for 220 to 240 minutes. After the heat preservation is completed, it is filtered and washed with deionized water for 4 to 6 times, and then dried at 70 to 72° C. for 50 to 60 minutes to obtain a dry product;

[0011] Wollastonite is ultrasonically dispersed in an appropriate amount of N,N-dimethylformamide at a solid-liquid ratio of 0.02-0.04 g / mL for 22-32 minutes, and then a dry product of 40-50% of the mass of wollastonite is added, and ultrasonic dispersion is continued for 50-60 minutes. Then, the mixture is heat-treated at 110-120°C for 350-370 minutes. After filtration, the mixture is washed with deionized water for 4-6 times and then dried at 70-72°C for 50-60 minutes to obtain modified carbon fiber.

[0012] The present invention is further configured as follows: the silane solution is prepared by mixing the composite material and deionized water at a solid-liquid ratio of 0.12 to 0.16 g / mL.

[0013] The present invention is further configured as follows: the compound material is formed by mixing 3-aminopropyltrimethoxysilane and γ-aminopropyltrimethoxysilane in a mass ratio of 0.3 to 0.6:1.

[0014] The present invention is further configured as follows: the preparation process of the graphene oxide polymer is as follows:

[0015] The graphene oxide was ultrasonically dispersed in an appropriate amount of 60-70% ethanol aqueous solution at a solid-liquid ratio of 0.12-0.22 g / mL for 20-30 minutes, and then polyetheramine PEA was added at 22-32% of the mass of the graphene oxide. The mixture was treated at 92-96° C. and 120-320 r / min for 350-370 minutes. After filtration, the mixture was washed with ethanol for 2-4 times and freeze-dried to obtain a graphene oxide base material.

[0016] Place an appropriate amount of polyurethane in an 80-82% ethanol aqueous solution at a solid-liquid ratio of 0.18-0.24 g / mL for 20-30 minutes to obtain a polyurethane solution;

[0017] An appropriate amount of graphene oxide base material is placed in a polyurethane solution at a solid-liquid ratio of 0.08 to 0.14 g / mL, and then 4-dimethylaminopyridine and N,N'-diisopropylcarbodiimide are added in sequence. The solution is treated at 90 to 100° C. for 120 to 130 minutes, then heated to 110 to 112° C. for 80 to 90 minutes. After filtration, the solution is washed with deionized water for 4 to 6 times, and then dried at 60 to 64° C. for 70 to 80 minutes to obtain a graphene oxide polymer.

[0018] The present invention is further configured as follows: the addition amount of the 4-dimethylaminopyridine is 2.2-5.2% of the mass of the graphene oxide base material, and the addition amount of the N,N'-diisopropylcarbodiimide is 2.5-5.5% of the mass of the graphene oxide base material.

[0019] The present invention is further configured such that: the lubricant is selected from any one of oxidized polyethylene wax and glyceryl stearate.

[0020] The present invention is further configured as follows: the antioxidant is selected from any one of antioxidant 164, antioxidant DNP, and antioxidant 1076.

[0021] The second aspect of the present invention further provides a method for preparing the composite material with low water absorption and water ripple appearance, comprising the following steps:

[0022] Step 1: Accurately weigh the modified carbon fiber, graphene oxide polymer, lubricant and antioxidant respectively, and then transfer the modified carbon fiber, graphene oxide polymer, lubricant and antioxidant into a mixing device for mixing for 20 to 30 minutes to obtain a mixed material;

[0023] Step 2: Add the obtained mixture into a twin-screw extruder, with the screw temperature ranging from 300 to 340° C. and the screw speed ranging from 250 to 300 r / min, and extrude and granulate to obtain a finished composite material.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The composite material prepared by the present invention uses modified carbon fibers, graphene oxide polymers, lubricants, and antioxidants as raw materials. The modified carbon fibers, graphene oxide polymers, lubricants, and antioxidants are weighed, then transferred into a mixing device for mixing, and finally extruded and granulated in a twin-screw extruder to produce a finished composite material. The prepared composite material not only has excellent low water absorption, but also has excellent tensile strength and flexural strength. The composite material prepared by the present invention has a broader market prospect and is more suitable for promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0027] Figure 1 Statistical graph of water absorption of the present invention;

[0028] Figure 2 Statistical diagram of the tensile strength of the present invention. DETAILED DESCRIPTION

[0029] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0030] Example 1

[0031] This embodiment provides a composite material with a low water absorption rate and a water-ripple appearance. The composite material is made of the following raw materials in parts by weight: 20 parts of modified carbon fiber, 8 parts of graphene oxide polymer, 10 parts of lubricant and 6 parts of antioxidant.

[0032] Among them, the preparation process of modified carbon fiber is as follows:

[0033] The chopped carbon fibers were ultrasonically dispersed in an appropriate amount of acetone at a solid-liquid ratio of 0.02 g / mL for 20 minutes. After the ultrasonic dispersion was completed, the resulting dispersion was treated in a 60°C water bath for 300 minutes, filtered, washed four times with deionized water, and then dried at 70°C for 50 minutes to obtain the carbon fibers.

[0034] The carbon fibers were ultrasonically dispersed in an appropriate amount of silane solution at a solid-liquid ratio of 0.05 g / mL for 30 minutes, and then heat-treated at 78°C for 220 minutes. After the heat-treatment, the mixture was filtered and washed four times with deionized water, and then dried at 70°C for 50 minutes to obtain a dry product.

[0035] Wollastonite was ultrasonically dispersed in an appropriate amount of N,N-dimethylformamide at a solid-liquid ratio of 0.02 g / mL for 22 minutes, and then a dry product of 40% of the mass of wollastonite was added, and ultrasonic dispersion was continued for 50 minutes. Then, the mixture was heat-treated at 110°C for 350 minutes. After filtration, the mixture was washed four times with deionized water and dried at 70°C for 50 minutes to obtain modified carbon fiber.

[0036] In this embodiment, it should be noted that the chopped carbon fibers were purchased from Shanghai Lishuo Composite Materials Technology Co., Ltd., and the wollastonite was purchased from Guangzhou Yifeng Chemical Technology Co., Ltd.

[0037] Furthermore, the silane solution is prepared by mixing the composite material and deionized water at a solid-liquid ratio of 0.12 g / mL.

[0038] Furthermore, the compound material is prepared by mixing 3-aminopropyltrimethoxysilane and γ-aminopropyltrimethoxysilane in a mass ratio of 0.3:1.

[0039] The preparation process of graphene oxide polymer is as follows:

[0040] Graphene oxide was ultrasonically dispersed in an appropriate amount of 60% ethanol aqueous solution at a solid-liquid ratio of 0.12 g / mL for 20 minutes, and then polyetheramine (PEA) was added at 22% by weight of the graphene oxide. The mixture was treated at 92°C and 120 rpm for 350 minutes. After filtration, the mixture was washed twice with ethanol and freeze-dried to obtain a graphene oxide base material.

[0041] An appropriate amount of polyurethane was placed in an 80% ethanol aqueous solution at a solid-liquid ratio of 0.18 g / mL for 20 minutes to obtain a polyurethane solution;

[0042] An appropriate amount of graphene oxide base material was placed in a polyurethane solution at a solid-liquid ratio of 0.08 g / mL, and 4-dimethylaminopyridine and N,N'-diisopropylcarbodiimide were added in sequence. The solution was treated at 90°C for 120 minutes, then heated to 110°C for 80 minutes. After filtration, the solution was washed four times with deionized water and dried at 60°C for 70 minutes to obtain a graphene oxide polymer.

[0043] Furthermore, the added amount of 4-dimethylaminopyridine is 2.2% of the mass of the graphene oxide base material, and the added amount of N,N'-diisopropylcarbodiimide is 2.5% of the mass of the graphene oxide base material.

[0044] In this embodiment, it should be noted that graphene oxide was purchased from Suzhou Beike Nanotechnology Co., Ltd., polyurethane TPU was purchased from Guangzhou Jingchen Plastics Co., Ltd., and polyetheramine PEA was purchased from Aladdin Reagent (Shanghai) Co., Ltd.

[0045] Among them, the lubricant is oxidized polyethylene wax.

[0046] The antioxidant used is antioxidant 164.

[0047] In addition, this embodiment also provides a method for preparing the composite material with low water absorption and water corrugated appearance, comprising the following steps:

[0048] Step 1: Accurately weigh the modified carbon fiber, graphene oxide polymer, lubricant and antioxidant respectively, and then transfer the modified carbon fiber, graphene oxide polymer, lubricant and antioxidant into a mixing device for mixing for 20 minutes to obtain a mixed material;

[0049] Step 2: Add the obtained mixture into a twin-screw extruder, with the screw temperature ranging from 300 to 340° C. and the screw speed at 250 r / min, and extrude and granulate to obtain a finished composite material.

[0050] This embodiment also provides a method for producing a three-dimensional water ripple appearance of a composite material with a planar effect, comprising the following steps:

[0051] 1) Mold Design: Design the concave and convex shape of the mold based on the desired water ripples. Design the mold depression starting from the edge of the water wave. Design the depth of the depression based on the number of layers of the corrugated surface corresponding to the number of carbon cloth (made of the composite material prepared in this embodiment) layers. The corners of the concave and convex shapes should be arc angles with a radius of not less than 0.5 mm and a maximum depth of not more than 3 mm. This will facilitate a fuller appearance and avoid missing shapes.

[0052] 2) Cutting: According to the requirements of the layup design, the rolled carbon cloth is first cut into large pieces and the relevant angles are combined. Then, an automatic cutting machine is used under computer control to cut the large pieces of carbon cloth into the required shape and size;

[0053] 3) Composite material: Lay the cut carbon cloth together according to the required thickness;

[0054] 4) Molding: The mixed carbon cloth is fixed in a mold, the mold is heated, and after a certain period of time, the resin in the carbon cloth is completely cured and then demolded to obtain a composite material blank;

[0055] Among them, the molding temperature is 80°C, the molding time is 10 minutes, and the molding pressure is 0.1 MPa.

[0056] 5) Finishing: Grind off the rough edge and cut around to the required size;

[0057] 6) Surface grinding: Install the rough blank on the surface grinding machine through a fixed fixture. Through repeated grinding, the highest point plane is required to be coplanar and the flatness is less than 0.5mm. The direction of the grain is fully displayed to achieve the desired water ripple size and three-dimensional effect;

[0058] 7) Re-grinding: Use transparent putty to fill the concave parts of the ground product, and then spray primer and polish the surface several times to make it smooth, with a flatness of less than 0.5mm;

[0059] 8) Painting: Spray high-gloss transparent paint according to product appearance requirements, and polish it several times to ensure the flatness is less than 0.5mm;

[0060] 9) Polishing: Use special equipment to polish the painted product to ensure that there is no sand, oil pits or pinholes on the surface.

[0061] Example 2

[0062] This embodiment provides a composite material with a low water absorption rate and a water-ripple appearance. The composite material is made of the following raw materials in parts by weight: 25 parts of modified carbon fiber, 10 parts of graphene oxide polymer, 15 parts of lubricant and 8 parts of antioxidant.

[0063] Among them, the preparation process of modified carbon fiber is as follows:

[0064] The chopped carbon fibers were ultrasonically dispersed in an appropriate amount of acetone at a solid-liquid ratio of 0.03 g / mL for 25 minutes. After the ultrasonic dispersion was completed, the resulting dispersion was treated in a 64°C water bath for 320 minutes, filtered, washed with deionized water five times, and then dried at 71°C for 55 minutes to obtain the carbon fibers.

[0065] The carbon fibers were ultrasonically dispersed in an appropriate amount of silane solution at a solid-liquid ratio of 0.06 g / mL for 35 minutes, and then heat-treated at 80°C for 230 minutes. After the heat-treatment, the mixture was filtered and washed five times with deionized water, and then dried at 71°C for 55 minutes to obtain a dry product.

[0066] Wollastonite was ultrasonically dispersed in an appropriate amount of N,N-dimethylformamide at a solid-liquid ratio of 0.03 g / mL for 26 minutes, and then a dry product of 45% of the mass of wollastonite was added, and ultrasonic dispersion was continued for 55 minutes. Then, the mixture was heat-treated at 115°C for 360 minutes. After filtration, the mixture was washed with deionized water 5 times and dried at 71°C for 55 minutes to obtain modified carbon fiber.

[0067] In this embodiment, it should be noted that the chopped carbon fibers were purchased from Shanghai Lishuo Composite Materials Technology Co., Ltd., and the wollastonite was purchased from Guangzhou Yifeng Chemical Technology Co., Ltd.

[0068] Furthermore, the silane solution was prepared by mixing the composite material and deionized water at a solid-liquid ratio of 0.14 g / mL.

[0069] Furthermore, the compound material is prepared by mixing 3-aminopropyltrimethoxysilane and γ-aminopropyltrimethoxysilane in a mass ratio of 0.4:1.

[0070] The preparation process of graphene oxide polymer is as follows:

[0071] Graphene oxide was ultrasonically dispersed in an appropriate amount of 65% ethanol aqueous solution at a solid-liquid ratio of 0.16 g / mL for 25 minutes, and then polyetheramine (PEA) was added at 26% of the mass of the graphene oxide. The mixture was treated at 94°C and 220 / min for 360 minutes. After filtration, the mixture was washed three times with ethanol and freeze-dried to obtain a graphene oxide base material.

[0072] A polyurethane solution was obtained by placing an appropriate amount of polyurethane in an 80-82% ethanol aqueous solution at a solid-liquid ratio of 0.21 g / mL for 25 minutes.

[0073] An appropriate amount of graphene oxide base material was placed in a polyurethane solution at a solid-liquid ratio of 0.12 g / mL, and 4-dimethylaminopyridine and N,N'-diisopropylcarbodiimide were added in sequence. The solution was treated at 95°C for 125 minutes, then heated to 111°C for 85 minutes. After filtration, the solution was washed with deionized water five times and dried at 62°C for 75 minutes to obtain a graphene oxide polymer.

[0074] Furthermore, the added amount of 4-dimethylaminopyridine is 3.2% of the mass of the graphene oxide base material, and the added amount of N,N'-diisopropylcarbodiimide is 3.5% of the mass of the graphene oxide base material.

[0075] In this embodiment, it should be noted that graphene oxide was purchased from Suzhou Beike Nanotechnology Co., Ltd., and polyurethane TPU was purchased from Guangzhou Jingchen Plastics Co., Ltd.

[0076] Among them, the lubricant is glyceryl stearate.

[0077] The antioxidant used is antioxidant DNP.

[0078] In addition, this embodiment also provides a method for preparing the composite material with low water absorption and water corrugated appearance, comprising the following steps:

[0079] Step 1: Accurately weigh the modified carbon fiber, graphene oxide polymer, lubricant and antioxidant respectively, and then transfer the modified carbon fiber, graphene oxide polymer, lubricant and antioxidant into a mixing equipment and mix them for 25 minutes to obtain a mixed material;

[0080] Step 2: Add the obtained mixture into a twin-screw extruder, with the screw temperature range of 320° C. and the screw speed of 270 r / min, and extrude and granulate to obtain a finished composite material.

[0081] This embodiment also provides a method for producing a three-dimensional water ripple appearance of a composite material with a planar effect, comprising the following steps:

[0082] 1) Mold Design: Design the concave and convex shape of the mold based on the desired water ripples. Design the mold depression starting from the edge of the water wave. Design the depth of the depression based on the number of layers of the corrugated surface corresponding to the number of carbon cloth (made of the composite material prepared in this embodiment) layers. The corners of the concave and convex shapes should be arc angles with a radius of not less than 0.5 mm and a maximum depth of not more than 3 mm. This will facilitate a fuller appearance and avoid missing shapes.

[0083] 2) Cutting: According to the requirements of the layup design, the rolled carbon cloth is first cut into large pieces and the relevant angles are combined. Then, an automatic cutting machine is used under computer control to cut the large pieces of carbon cloth into the required shape and size;

[0084] 3) Composite material: Lay the cut carbon cloth together according to the required thickness;

[0085] 4) Molding: The mixed carbon cloth is fixed in a mold, the mold is heated, and after a certain period of time, the resin in the carbon cloth is completely cured and then demolded to obtain a composite material blank;

[0086] The molding temperature is 100°C, the molding time is 70 min, and the molding pressure is 0.5 MPa.

[0087] 5) Finishing: Grind off the rough edge and cut around to the required size;

[0088] 6) Surface grinding: Install the rough blank on the surface grinding machine through a fixed fixture. Through repeated grinding, the highest point plane is required to be coplanar and the flatness is less than 0.5mm. The direction of the grain is fully displayed to achieve the desired water ripple size and three-dimensional effect;

[0089] 7) Re-grinding: Use transparent putty to fill the concave parts of the ground product, and then spray primer and polish the surface several times to make it smooth, with a flatness of less than 0.5mm;

[0090] 8) Painting: Spray high-gloss transparent paint according to product appearance requirements, and polish it several times to ensure the flatness is less than 0.5mm;

[0091] 9) Polishing: Use special equipment to polish the painted product to ensure that there is no sand, oil pits or pinholes on the surface.

[0092] Example 3

[0093] This embodiment provides a composite material with a low water absorption rate and a water-ripple appearance. The composite material is made of the following raw materials in parts by weight: 30 parts of modified carbon fiber, 12 parts of graphene oxide polymer, 20 parts of lubricant and 10 parts of antioxidant.

[0094] Among them, the preparation process of modified carbon fiber is as follows:

[0095] The chopped carbon fibers were ultrasonically dispersed in an appropriate amount of acetone at a solid-liquid ratio of 0.05 g / mL for 30 minutes. After the ultrasonic dispersion was completed, the resulting dispersion was treated in a 68°C water bath for 340 minutes, filtered, washed with deionized water 6 times, and then dried at 72°C for 60 minutes to obtain the carbon fibers.

[0096] The carbon fibers were ultrasonically dispersed in an appropriate amount of silane solution at a solid-liquid ratio of 0.07 g / mL for 40 minutes, and then heat-treated at 82°C for 240 minutes. After the heat-treatment, the mixture was filtered and washed with deionized water six times, and then dried at 72°C for 60 minutes to obtain a dry product.

[0097] Wollastonite was ultrasonically dispersed in an appropriate amount of N,N-dimethylformamide at a solid-liquid ratio of 0.04 g / mL for 32 minutes, and then a dry product of 50% of the mass of wollastonite was added, and ultrasonic dispersion was continued for 60 minutes. Then, the mixture was heat-treated at 120°C for 370 minutes. After filtration, the mixture was washed with deionized water 6 times and then dried at 72°C for 60 minutes to obtain modified carbon fiber.

[0098] In this embodiment, it should be noted that the chopped carbon fibers were purchased from Shanghai Lishuo Composite Materials Technology Co., Ltd., and the wollastonite was purchased from Guangzhou Yifeng Chemical Technology Co., Ltd.

[0099] Furthermore, the silane solution was prepared by mixing the composite material and deionized water at a solid-liquid ratio of 0.16 g / mL.

[0100] Furthermore, the compound material is prepared by mixing 3-aminopropyltrimethoxysilane and γ-aminopropyltrimethoxysilane in a mass ratio of 0.6:1.

[0101] The preparation process of graphene oxide polymer is as follows:

[0102] Graphene oxide was ultrasonically dispersed in an appropriate amount of 70% ethanol aqueous solution at a solid-liquid ratio of 0.22 g / mL for 30 minutes, and then polyetheramine (PEA) with a concentration of 32% of the mass of graphene oxide was added. The mixture was treated at 96°C and 320 rpm for 370 minutes. After filtration, the mixture was washed four times with ethanol and freeze-dried to obtain a graphene oxide base material.

[0103] An appropriate amount of polyurethane was placed in an 82% ethanol aqueous solution at a solid-liquid ratio of 0.24 g / mL for 30 minutes to obtain a polyurethane solution;

[0104] An appropriate amount of graphene oxide base material was placed in a polyurethane solution at a solid-liquid ratio of 0.14 g / mL, and 4-dimethylaminopyridine and N,N'-diisopropylcarbodiimide were added in sequence. The solution was treated at 100°C for 130 minutes, then heated to 112°C for 90 minutes. After filtration, the solution was washed with deionized water six times and then dried at 64°C for 80 minutes to obtain a graphene oxide polymer.

[0105] Furthermore, the added amount of 4-dimethylaminopyridine is 5.2% of the mass of the graphene oxide base material, and the added amount of N,N'-diisopropylcarbodiimide is 5.5% of the mass of the graphene oxide base material.

[0106] In this embodiment, it should be noted that graphene oxide was purchased from Suzhou Beike Nanotechnology Co., Ltd., and polyurethane TPU was purchased from Guangzhou Jingchen Plastics Co., Ltd.

[0107] Among them, the lubricant is oxidized polyethylene wax.

[0108] Antioxidant 1076 was selected as the antioxidant.

[0109] In addition, this embodiment also provides a method for preparing the composite material with low water absorption and water corrugated appearance, comprising the following steps:

[0110] Step 1: Accurately weigh the modified carbon fiber, graphene oxide polymer, lubricant and antioxidant respectively, and then transfer the modified carbon fiber, graphene oxide polymer, lubricant and antioxidant into a mixing device for mixing for 30 minutes to obtain a mixed material;

[0111] Step 2: Add the obtained mixture into a twin-screw extruder, with the screw temperature ranging from 300 to 340° C. and the screw speed being 300 r / min, and extrude and granulate to obtain a finished composite material.

[0112] This embodiment also provides a method for producing a three-dimensional water ripple appearance of a composite material with a planar effect, comprising the following steps:

[0113] 1) Mold Design: Design the concave and convex shape of the mold based on the desired water ripples. Design the mold depression starting from the edge of the water wave. Design the depth of the depression based on the number of layers of the corrugated surface corresponding to the number of carbon cloth (made of the composite material prepared in this embodiment) layers. The corners of the concave and convex shapes should be arc angles with a radius of not less than 0.5 mm and a maximum depth of not more than 3 mm. This will facilitate a fuller appearance and avoid missing shapes.

[0114] 2) Cutting: According to the requirements of the layup design, the rolled carbon cloth is first cut into large pieces and the relevant angles are combined. Then, an automatic cutting machine is used under computer control to cut the large pieces of carbon cloth into the required shape and size;

[0115] 3) Composite material: Lay the cut carbon cloth together according to the required thickness;

[0116] 4) Molding: The mixed carbon cloth is fixed in a mold, the mold is heated, and after a certain period of time, the resin in the carbon cloth is completely cured and then demolded to obtain a composite material blank;

[0117] The molding temperature is 130°C, the molding time is 120 min, and the molding pressure is 1.0 MPa.

[0118] 5) Finishing: Grind off the rough edge and cut around to the required size;

[0119] 6) Surface grinding: Install the rough blank on the surface grinding machine through a fixed fixture. Through repeated grinding, the highest point plane is required to be coplanar and the flatness is less than 0.5mm. The direction of the grain is fully displayed to achieve the desired water ripple size and three-dimensional effect;

[0120] 7) Re-grinding: Use transparent putty to fill the concave parts of the ground product, and then spray primer and polish the surface several times to make it smooth, with a flatness of less than 0.5mm;

[0121] 8) Painting: Spray high-gloss transparent paint according to product appearance requirements, and polish it several times to ensure the flatness is less than 0.5mm;

[0122] 9) Polishing: Use special equipment to polish the painted product to ensure that there is no sand, oil pits or pinholes on the surface.

[0123] Comparative Example 1: The preparation method of the composite material provided in this embodiment and the specific ratio of raw materials are roughly the same as those in Example 1, with the main difference being that the modified carbon fiber in this embodiment is replaced by carbon fiber.

[0124] Comparative Example 2: The preparation method of the composite material and the specific ratio of raw materials provided in this embodiment are substantially the same as those in Example 1, with the main difference being that wollastonite is not added to the modified carbon fiber in this embodiment.

[0125] Comparative Example 3: The preparation method of the composite material provided in this embodiment and the specific ratio of raw materials are substantially the same as those in Example 1, with the main difference being that the graphene oxide base material in this embodiment is replaced by graphene oxide.

[0126] Effect test

[0127] The composite materials prepared by Examples 1 to 3 of the present invention are respectively recorded as Experimental Examples 1 to 3; the composite materials prepared by Comparative Examples 1 to 3 are respectively recorded as Comparative Examples 1 to 3; and then the properties of equal amounts of composite material samples in each group are respectively tested.

[0128] Test 1. Water absorption test and result analysis:

[0129] The water absorption of each group of composite materials was tested according to the test standard of GB / T 1034-2008 (23°C, i.e., Method 1), and the relevant data are recorded in Table 1.

[0130] Table 1: Test data record table

[0131] Group Water absorption (%) Example 1 group 0.1 Example 2 group 0.1 Example 3 group 0.1 Comparison group 1 0.4 Comparison of 2 groups 0.3 Comparison of 3 groups 0.3

[0132] From Table 1 and Figure 1 It can be seen that compared with the control group, the composite materials of Examples 1 to 3 can significantly reduce water absorption; at the same time, the differences between the various example groups are not obvious. The above results show that the composite materials of Examples 1 to 3 have a significant effect of reducing water absorption.

[0133] In order to verify the effects of the various components of the additive, experiments of Comparative Examples 1 to 3 were set up.

[0134] The main difference in the raw material ratio between the composite materials of Comparative Group 1 and Example 1 is that the modified carbon fiber is replaced by carbon fiber. Compared with Example 1, the water absorption rate of the Comparative Group 1 increased by 0.3%. This result shows that the modified carbon fiber plays an important role in reducing the water absorption rate of the composite material.

[0135] The main difference in the raw material ratios between the composite materials in Comparative Group 2 and Example 1 is that wollastonite was not added to the modified carbon fibers. Compared to Example 1, the water absorption rate in Comparative Group 2 increased by 20%. This result suggests that wollastonite has a certain effect in reducing the water absorption rate of composite materials.

[0136] The main difference in the raw material ratio between the composite materials in Comparative Group 3 and Example 1 is that the graphene oxide base material is replaced by graphene oxide. Compared with Example 1, the water absorption rate of Comparative Group 3 increased by 0.2%. This result indicates that the graphene oxide base material has a certain effect on reducing the water absorption rate of the composite material.

[0137] Test 2: Mechanical properties test and result analysis:

[0138] The tensile properties are tested according to the testing standard GB / T1040-2018, and the bending properties are tested according to the testing standard GB / T9341-2008.

[0139] Table 2: Experimental data record table

[0140] Group Tensile strength (MPa) Flexural strength (MPa) Example 1 group 200 305 Example 2 group 195 300 Example 3 group 195 300 Comparison group 1 125 270 Comparison of 2 groups 135 285 Comparison of 3 groups 140 290

[0141] From Table 2 and Figure 2 It can be seen that compared with the control group, the composite materials of Examples 1 to 3 can significantly enhance the tensile strength and flexural strength; at the same time, the differences between the various example groups are not significant. The above results show that the composite materials of Examples 1 to 3 have excellent mechanical properties.

[0142] In order to verify the effects of the various components of the additive, experiments of Comparative Examples 1 to 3 were set up.

[0143] The main difference in the raw material ratio between the composite materials of Comparative Group 1 and Example 1 is that the modified carbon fibers are replaced by carbon fibers. Compared with Example 1, the tensile strength of the Comparative Group 1 decreased by 75 MPa and the flexural strength decreased by 35 MPa. These results indicate that the modified carbon fibers play a significant role in enhancing the tensile and flexural strength of the composite materials.

[0144] The main difference in the raw material ratios between the composite materials in Comparative Group 2 and Example 1 is the omission of wollastonite in the modified carbon fibers. Compared to Example 1, the tensile strength of Comparative Group 2 decreased by 65 MPa and the flexural strength decreased by 20 MPa. These results suggest that wollastonite plays a role in enhancing the tensile and flexural strength of the composite materials.

[0145] The main difference in the raw material ratios between the composites in Comparative Group 3 and Example 1 was that the graphene oxide matrix was replaced with graphene oxide. Compared to Example 1, the tensile strength of Comparative Group 3 decreased by 60 MPa and the flexural strength decreased by 15 MPa. These results indicate that the graphene oxide matrix contributes to the enhanced tensile and flexural strength of the composites.

[0146] As can be seen from the above, the composite material prepared by the present invention not only has excellent low water absorption effect, but also has excellent tensile strength and flexural strength. This shows that the composite material produced by the present invention has a broader market prospect and is more suitable for promotion.

[0147] Throughout this specification, references to terms such as "one embodiment," "example," or "specific example" indicate that the specific features, structures, materials, or characteristics described in conjunction with that embodiment or example are included in at least one embodiment or example of the present invention. In this specification, schematic representations of these terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in any one or more embodiments or examples.

[0148] The preferred embodiments of the present invention disclosed above are intended only to help illustrate the present invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the present invention to the specific embodiments described. Obviously, many modifications and variations are possible based on the content of this specification. These embodiments are selected and described in detail in this specification to better explain the principles and practical applications of the present invention, thereby enabling those skilled in the art to better understand and utilize the present invention. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A composite material with low water absorption and water ripple appearance, Features: The composite material is made of the following raw materials in parts by weight: 20 to 30 parts of modified carbon fiber, 8 to 12 parts of graphene oxide polymer, 10 to 20 parts of lubricant and 6 to 10 parts of antioxidant; The preparation process of the modified carbon fiber is as follows: The short-cut carbon fiber is ultrasonically dispersed in an appropriate amount of acetone at a solid-liquid ratio of 0.02 to 0.05 g / mL for 20 to 30 minutes; after the ultrasonic dispersion is completed, the obtained dispersion is treated in a water bath at 60 to 68°C for 300 to 340 minutes, filtered, washed with deionized water for 4 to 6 times, and then dried at 70 to 72°C for 50 to 60 minutes to obtain the carbon fiber; The carbon fiber is ultrasonically dispersed in an appropriate amount of silane solution at a solid-liquid ratio of 0.05-0.07 g / mL for 30-40 minutes, and then heat-treated at 78-82°C for 220-240 minutes. After the heat-insulation is completed, it is filtered and washed with deionized water for 4-6 times, and then dried at 70-72°C for 50-60 minutes to obtain a dry product; The wollastonite was ultrasonically dispersed in an appropriate amount of N,N-dimethylformamide at a solid-liquid ratio of 0.02-0.04 g / mL for 22-32 minutes, and then a dry product of 40-50% of the mass of the wollastonite was added, and the ultrasonic dispersion was continued for 50-60 minutes, and then the mixture was heat-treated at 110-120° C. for 350-370 minutes, and after filtration, the mixture was washed with deionized water for 4-6 times, and then dried at 70-72° C. for 50-60 minutes to obtain a modified carbon fiber; The preparation process of the graphene oxide polymer is as follows: The graphene oxide is ultrasonically dispersed in an appropriate amount of 60-70% ethanol aqueous solution at a solid-liquid ratio of 0.12-0.22 g / mL for 20-30 min, and then 22-32% of the mass of the graphene oxide is added with polyetheramine PEA, and the mixture is treated at 92-96° C. and 120-320 r / min for 350-370 min. After suction filtration, the mixture is washed with ethanol for 2-4 times, and then freeze-dried to obtain a graphene oxide base material; Place an appropriate amount of polyurethane in an ethanol aqueous solution with a concentration of 80 to 82% at a solid-liquid ratio of 0.18 to 0.24 g / mL for 20 to 30 minutes to obtain a polyurethane solution; An appropriate amount of graphene oxide base material is placed in a polyurethane solution at a solid-liquid ratio of 0.08-0.14 g / mL, and 4-dimethylaminopyridine and N,N'-diisopropylcarbodiimide are added in sequence, and the solution is treated at 90-100° C. for 120-130 min, and then the solution is heated to 110-112° C. for 80-90 min. After filtration, the solution is washed with deionized water for 4-6 times, and then dried at 60-64° C. for 70-80 min to obtain a graphene oxide polymer.

2. According to the composite material with low water absorption and water ripple appearance as claimed in claim 1, Features: The silane solution is prepared by mixing compound materials and deionized water at a solid-liquid ratio of 0.12 to 0.16 g / mL.

3. According to the composite material with low water absorption and water ripple appearance as claimed in claim 1, Features: The added amount of the 4-dimethylaminopyridine is 2.2-5.2% of the mass of the graphene oxide base material, and the added amount of the N,N'-diisopropylcarbodiimide is 2.5-5.5% of the mass of the graphene oxide base material.

4. According to the composite material with low water absorption and water ripple appearance as claimed in claim 1, Features: The lubricant is selected from any one of oxidized polyethylene wax and stearic acid glyceryl ester.

5. According to the composite material with low water absorption and water ripple appearance as claimed in claim 1, Features: The antioxidant is selected from any one of antioxidant 164, antioxidant DNP, and antioxidant 1076.

6. A method for preparing a composite material with a low water absorption rate and a water ripple appearance according to any one of claims 1 to 5, It is characterized in that The following steps are involved: Step 1, accurately weighing the modified carbon fiber, graphene oxide polymer, lubricant and antioxidant respectively, and then transferring the modified carbon fiber, graphene oxide polymer, lubricant and antioxidant into a mixing device for mixing for 20 to 30 minutes to obtain a mixed material; Step 2: Add the obtained mixed material into a twin-screw extruder, with the screw temperature ranging from 300 to 340° C. and the screw speed ranging from 250 to 300 r / min, and extrude and granulate to obtain a finished composite material.