A weather-resistant coating for transparent PC cover of new energy vehicle headlights and preparation method thereof
By using a weather-resistant coating containing specially modified acrylic resin and other additives on the headlights of new energy vehicles, the problem of aging of transparent PC cover of the headlights is solved, and the hardness and high temperature resistance are similar to that of glass are achieved, and the lengthening of the length of the glass is extended. Lifespan and reduce replacement costs.
Patent Information
- Application Number
- CN202410679246.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-05-29
AI Technical Summary
The transparent PC cover of the exterior light of new energy vehicles is prone to aging such as yellowing, blurring, cracking and other aging phenomena during use, resulting in a decrease in photoresistance and aging performance, increasing replacement costs and causing waste of resources.
Using a weather-resistant coating including specially modified acrylic resin, leveling agent, substrate wetting agent, ultraviolet absorber, light stabilizer, antioxidant and solvent, the modified acrylic resin is prepared by preparing nano-carbon silicon material and by Specific stirring and filtration steps are used to prepare coatings with Si-O and Si-C chemical bonds to achieve similar hardness and high temperature resistance to glass.
The coating is fully cured after baking at 800°C for 60-90 minutes, and has an ultra-long photo-aging performance. Due to the existence of Si-C chemical bonds, the paint film has good flexibility and is better than traditional UV coatings, which reduces the Replacement costs and reduce resource waste.
Smart Images

Figure CN118440546B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of coatings for exterior lamps of new energy vehicles, and in particular to a weather-resistant coating for a transparent PC cover of a lamp of a new energy vehicle and a preparation method thereof. Background Art
[0002] In recent years, with the rapid popularization of new energy vehicles in China, the requirements for the decoration of new energy vehicles' interior and exterior are getting higher and higher, especially in the field of exterior lights, where various through-type headlights emerge in an endless stream. Due to the need to provide various customized requirements, transparent PC as the main substrate, combined with double-sided coating technology and laser engraving technology, has gradually become the mainstream technology for new energy vehicle exterior lights.
[0003] Traditional car lights are limited to the headlight or taillight area and do not require processing on both sides, so traditional weather-resistant UV coatings can be used. The hardness of the PC cover is determined by the UV coating sprayed on its surface. After a certain number of years of use, the cover of the car headlight will show aging phenomena such as yellowing, blurring, and cracking, resulting in a decrease in light aging performance under long-term use, which has a great impact on the safe driving and appearance of the vehicle. For safety reasons, the car headlights need to be replaced. If replaced, the entire car headlight assembly must be replaced, including the original bulbs and reflective cups that can still be used normally. The replacement cost is high and causes a certain waste of resources. Summary of the invention
[0004] The purpose of the present invention is to provide a weather-resistant coating for a transparent PC cover of a new energy vehicle lamp and a preparation method thereof, so as to solve the deficiencies in the prior art.
[0005] To achieve the above object, the present invention provides the following solutions:
[0006] A weather-resistant coating for a transparent PC cover of a new energy vehicle lamp, the weather-resistant coating comprising: by weight, 55-75 parts of a special modified acrylic resin, 0.5-1 parts of a leveling agent, 0.5-1 parts of a substrate wetting agent, 1-3 parts of an ultraviolet absorber, 1-3 parts of a light stabilizer, 1-3 parts of an antioxidant and 10-35 parts of a solvent.
[0007] Preferably, the special modified acrylic resin is a homemade nano-carbon silicon material modified acrylic resin.
[0008] Preferably, the leveling agent is one of TegoWet450 and BYK333 produced by Evonik Chemicals.
[0009] Preferably, the substrate wetting agent is one of TegoWet270 and Twin4100 produced by Evonik Chemicals.
[0010] Preferably, the model of the ultraviolet absorber is one or more of Tinuvin1130 and Tinuvin400.
[0011] Preferably, the light stabilizer is one or more of Tinuvin292 and Tinuvin123.
[0012] Preferably, the antioxidant is one or more of the hindered phenol antioxidants irganox1010, irganox1076 and the phosphite antioxidants Irgafos168, Zhiyi 3010.
[0013] Preferably, the solvent is one or more of propylene glycol methyl ether acetate, n-butyl acetate, and ethyl acetate.
[0014] The present invention also provides a method for preparing a weather-resistant coating for a transparent PC cover of a new energy vehicle lamp, comprising the following steps:
[0015] S1, preparing nano-carbon silicon material modified acrylic resin;
[0016] S2, adding ultraviolet absorber, light stabilizer, antioxidant and part of solvent into the paint making tank, stirring evenly to obtain a premix;
[0017] S3, adding the nano-carbon silicon material modified acrylic resin obtained in step S1 and the remaining solvent in step S2 to the premix, adding a leveling agent and a substrate wetting agent to the paint making tank in sequence at a speed of 800-1000 rpm / min, stirring evenly, to obtain a mixture;
[0018] S4, adding a mixed solvent to the mixture obtained in step S3, adjusting the viscosity of the mixture to 8-9s, and then filtering through a 400-mesh filter to obtain a finished coating product.
[0019] Preferably, in step S1, the preparation process of the nano-carbon silicon material modified acrylic resin is as follows: add an organic solvent and a caprolactone solution to a stainless steel reactor respectively and stir evenly, then heat the stainless steel reactor to a reflux state, and control the temperature between 125 and 145° C.; then dropwise add a mixed solvent, and control the addition of the mixed solvent after 2 to 3 hours, and keep the temperature for 1 to 2 hours to react, then add an initiator to the stainless steel reactor, and after keeping the temperature for 2 to 3 hours, put the remaining organic solvent into the stainless steel reactor for reaction, and after the reaction is completed, cool the stainless steel reactor to 70 to 80° C., adjust the solid content and viscosity of the reaction solution, and filter and discharge to obtain the nano-carbon silicon material modified acrylic resin;
[0020] The mixed solvent consists of methacrylates, acrylates, organic silane and initiator.
[0021] According to the specific embodiments provided by the present invention, the present invention discloses the following technical effects:
[0022] The invention provides a weather-resistant coating for a transparent PC cover of a new energy vehicle lamp and a preparation method thereof. The coating can be fully cured by baking at 80°C for 60-90 minutes. After curing into a film, there are only two chemical bonds, Si-O and Si-C, in the molecular structure. The chemical composition is similar to that of quartz glass, and the hardness, high temperature resistance and various other chemical medium resistance properties similar to those of glass can be achieved. In addition, the prepared weather-resistant coating can achieve ultra-long-term light aging resistance in the application of outdoor products. At the same time, because it has a special Si-C chemical bond, the paint film can have good flexibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0024] Figure 1 The present invention is a flow chart of a method for preparing a weather-resistant coating for a transparent PC cover of a new energy vehicle lamp. DETAILED DESCRIPTION
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0027] like Figure 1 As shown, the present invention provides a method for preparing a weather-resistant coating for a transparent PC cover of a new energy vehicle lamp, comprising the following steps:
[0028] S1, preparing nano-carbon silicon material modified acrylic resin;
[0029] Wherein, in step S1, the preparation process of nano-carbon silicon material modified acrylic resin is as follows: add organic solvent and caprolactone solution to a stainless steel reactor respectively and stir evenly, then heat the stainless steel reactor to reflux state, and control the temperature between 125 and 145°C; then dropwise add mixed solvent, control the addition of mixed solvent after 2 to 3 hours, keep warm for 1 to 2 hours to react, then add initiator to the stainless steel reactor, keep warm for 2 to 3 hours, put the remaining organic solvent into the stainless steel reactor for reaction, cool the stainless steel reactor to 70 to 80°C after the reaction, adjust the solid content and viscosity of the reaction solution, and filter and discharge to obtain nano-carbon silicon material modified acrylic resin;
[0030] In addition, the mixed solvent is composed of methacrylates, acrylates, organic silane and initiator.
[0031] S2, adding ultraviolet absorber, light stabilizer, antioxidant and part of solvent into the paint making tank, stirring evenly to obtain a premix;
[0032] S3, adding the nano-carbon silicon material modified acrylic resin obtained in step S1 and the remaining solvent in step S2 to the premix, adding a leveling agent and a substrate wetting agent to the paint making tank in sequence at a speed of 800-1000 rpm / min, stirring evenly, to obtain a mixture;
[0033] S4, adding a mixed solvent to the mixture obtained in step S3, adjusting the viscosity of the mixture to 8-9s, and then filtering through a 400-mesh filter to obtain a finished coating product.
[0034] Specifically, the formula of the weather-resistant coating is, by weight, 55 to 75 parts of a special modified acrylic resin, 0.5 to 1 parts of a leveling agent, 0.5 to 1 parts of a substrate wetting agent, 1 to 3 parts of an ultraviolet absorber, 1 to 3 parts of a light stabilizer, 1 to 3 parts of an antioxidant and 10 to 35 parts of a solvent.
[0035] Among them, the special modified acrylic resin is a homemade nano-carbon silicon material modified acrylic resin. The model of the leveling agent is one of Evonik Chemical TegoWet450 and BYK333, and the leveling agents are purchased from Jiangmen Dongyang Chemical Co., Ltd. The model of the substrate wetting agent is one of Evonik Chemical TegoWet270 and Twin4100, and the substrate wetting agents are purchased from Foshan Shunde Sansheng Trading Co., Ltd. The model of the ultraviolet absorber is one or more of Tinuvin1130 and Tinuvin400; the model of the light stabilizer is one or more of Tinuvin292 and Tinuvin123, and the ultraviolet absorber and the light stabilizer are purchased from BASF Chemical in Germany. The model of the antioxidant is one or more of the hindered phenol antioxidant irganox1010, irganox1076 and the phosphite antioxidant Irgafos168, Zhiyi 3010, and the antioxidant is purchased from Shanghai Kaiyin Chemical. The solvent is one or more of propylene glycol methyl ether acetate, n-butyl acetate and ethyl acetate.
[0036] Example 1
[0037] In this embodiment, the formula of the weather-resistant coating is calculated by weight: 55 parts of special modified acrylic resin, 1 part of leveling agent, 1 part of substrate wetting agent, 3 parts of ultraviolet absorber, 3 parts of light stabilizer, 2 parts of antioxidant and 35 parts of solvent. The weather-resistant coating is prepared by the above preparation method.
[0038] Example 2
[0039] Different from Example 1, the formula of the weather-resistant coating is calculated by weight: 65 parts of special modified acrylic resin, 0.5 parts of leveling agent, 0.5 parts of substrate wetting agent, 2 parts of ultraviolet absorber, 2 parts of light stabilizer, 1 part of antioxidant and 29 parts of solvent.
[0040] Example 3
[0041] Different from Example 1, the formula of the weather-resistant coating is calculated by weight: 75 parts of special modified acrylic resin, 0.5 parts of leveling agent, 0.5 parts of substrate wetting agent, 1 part of ultraviolet absorber, 1 part of light stabilizer, 2 parts of antioxidant and 20 parts of solvent.
[0042] Example 4
[0043] Different from Example 1, the formula of the weather-resistant coating is calculated by weight: 60 parts of special modified acrylic resin, 1 part of leveling agent, 1 part of substrate wetting agent, 3 parts of ultraviolet absorber, 3 parts of light stabilizer, 3 parts of antioxidant and 29 parts of solvent.
[0044] Finally, the performance of the weather-resistant coatings prepared in Examples 1 to 4 and the traditional weather-resistant UV coatings for vehicle lamps were tested, and the results shown in Table 1 were obtained.
[0045] Table 1 Performance test indicators
[0046] ;
[0047] According to the test results in Table 1, the weather-resistant coatings prepared in Examples 1 to 4 have no obvious scratches after 200 dry grindings, but the traditional UV coatings have obvious scratches after 200 dry grindings. In addition, the water contact angles of the weather-resistant coatings prepared in Examples 1 to 4 are all greater than 105°, while the water contact angles of the traditional UV coatings are only between 85° and 95°, which proves that the performance of the weather-resistant coatings prepared in Examples 1 to 4 is better than that of the traditional UV coatings; and the hardness of the weather-resistant coatings in Examples 1 to 4 is better than that of the traditional UV coatings, which shows that after the weather-resistant coatings prepared in Examples 1 to 4 are cured into films, there are only two chemical bonds, Si-O and Si-C, in their molecular structures, and their chemical composition is similar to that of quartz glass, which can achieve hardness, high temperature resistance and various other chemical medium resistance characteristics similar to those of glass. At the same time, through the xenon arc lamp aging test, it can be found that the weather-resistant coatings prepared in Examples 1 to 4 have better aging resistance than traditional UV coatings.
[0048] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0049] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core idea of the present invention. At the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A weather-resistant coating for transparent PC cover of new energy vehicle headlights, characterized in that: The weather-resistant coating comprises: by weight, 55-75 parts of a special modified acrylic resin, 0.5-1 parts of a leveling agent, 0.5-1 parts of a substrate wetting agent, 1-3 parts of an ultraviolet absorber, 1-3 parts of a light stabilizer, 1-3 parts of an antioxidant and 10-35 parts of a solvent; the coating can be fully cured by baking at 80° C. for 60-90 minutes; The preparation method of the weather-resistant coating comprises the following steps: S1, preparing nano-carbon silicon material modified acrylic resin; S2, adding ultraviolet absorber, light stabilizer, antioxidant and part of solvent into the paint making tank, stirring evenly to obtain a premix; S3, adding the nano-carbon silicon material modified acrylic resin obtained in step S1 and the remaining solvent in step S2 to the premix, adding a leveling agent and a substrate wetting agent to the paint making tank in sequence at a speed of 800-1000 rpm / min, stirring evenly, to obtain a mixture; S4, adding a mixed solvent to the mixture obtained in step S3, adjusting the viscosity of the mixture to 8-9s, and then filtering through a 400-mesh filter to obtain a finished coating product; In step S1, the preparation process of the nano-carbon silicon material modified acrylic resin is as follows: add an organic solvent and a caprolactone solution to a stainless steel reactor respectively and stir evenly, then heat the stainless steel reactor to a reflux state, and control the temperature between 125 and 145° C.; then drop a mixed solvent, control the addition of the mixed solvent after 2 to 3 hours, keep the temperature for 1 to 2 hours to react, then add an initiator to the stainless steel reactor, keep the temperature for 2 to 3 hours, put the remaining organic solvent into the stainless steel reactor for reaction, and after the reaction is completed, cool the stainless steel reactor to 70 to 80° C., adjust the solid content and viscosity of the reaction solution, and filter and discharge to obtain the nano-carbon silicon material modified acrylic resin; The mixed solvent consists of methacrylates, acrylates, organic silane and initiator.
2. The weather-resistant coating for transparent PC cover of new energy vehicle headlights according to claim 1 is characterized in that: The model of the leveling agent is one of Evonik Chemicals' TegoWet450 and BYK333.
3. The weather-resistant coating for transparent PC cover of new energy vehicle headlights according to claim 1 is characterized in that: The model of the substrate wetting agent is one of Evonik Chemicals' TegoWet270 and Twin4100.
4. The weather-resistant coating for transparent PC cover of new energy vehicle headlights according to claim 1, characterized in that: The model of the ultraviolet absorber is one or more of Tinuvin1130 and Tinuvin400.
5. The weather-resistant coating for transparent PC cover of new energy vehicle headlights according to claim 1, characterized in that: The light stabilizer may be one or more of Tinuvin292 and Tinuvin123.
6. The weather-resistant coating for transparent PC cover of new energy vehicle headlights according to claim 1, characterized in that: The antioxidant is selected from one or more of the hindered phenol antioxidants irganox1010 and irganox1076 and the phosphite antioxidants Irgafos168 and Zhiyi 3010.
7. The weather-resistant coating for transparent PC cover of new energy vehicle headlights according to claim 1 is characterized in that: The solvent is one or more of propylene glycol methyl ether acetate, n-butyl acetate, and ethyl acetate.