A ceramic diaphragm with stable safety and preparation method thereof

By coating the fluorinated aramid polymer coating liquid on the ceramic separator, a ceramic composite separator with high bonding performance and safety performance is formed, which solves the problem of insufficient safety performance of traditional ceramic separators and improves the safety performance of lithium-ion batteries. .

CN118448814BActive Publication Date: 2024-10-29CANGZHOU MINGZHU SEPARATOR TECH CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410691953.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-31
Publication Date
2024-10-29
Estimated Expiration
2044-05-31

AI Technical Summary

Technical Problem

Traditional ceramic separators have insufficient safety performance due to heat accumulation during the charging and discharging process of lithium-ion batteries, and there are potential safety hazards.

Method used

The polymer coating liquid with fluorinated aramid is coated on the surface of the ceramic separator, and is solidified and dried through a specific preparation method to form a ceramic composite separator with higher bonding performance and safety performance.

Benefits of technology

It significantly improves the membrane rupture temperature and bonding performance of the ceramic composite diaphragm, enhances its safety performance, and avoids safety threats caused by heat accumulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The present invention relates to the field of diaphragm technology, and specifically to a ceramic composite diaphragm with stability and safety and a preparation method thereof. The ceramic composite diaphragm with stability and safety of the present invention comprises a ceramic diaphragm and a polymer coating located on the surface of the ceramic diaphragm, wherein the polymer coating is obtained by coating a polymer coating liquid on the surface of the ceramic diaphragm, curing it in a coagulation bath, washing it with water, and drying it; the polymer coating liquid contains fluorinated aramid. Compared with traditional ceramic diaphragms, its membrane breaking temperature is significantly improved, which can effectively improve the high temperature resistance of the diaphragm above 150°C and the bonding performance between the diaphragm and the pole piece, while improving the pass rate of the hot needle puncture of the battery, thereby effectively improving the safety performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of diaphragms, and in particular to a ceramic diaphragm with stability and safety and a preparation method thereof. Background Art

[0002] Lithium-ion batteries are rechargeable batteries that are widely used in mobile devices, electric vehicles, energy storage systems, and other fields. Lithium-ion batteries store and release charges by the migration of lithium ions between the positive and negative electrodes. They have the advantages of high energy density, long cycle life, low self-discharge rate, and environmental protection. Therefore, they have become one of the most common and widely used types of rechargeable batteries. With the advancement of technology, the performance of lithium-ion batteries has been continuously improved and they are widely used in various fields.

[0003] The main components of lithium-ion batteries include positive electrode, negative electrode, electrolyte and separator. Among them, the separator is an important component in lithium-ion batteries. The separator should have sufficient ion permeability so that lithium ions can be smoothly transmitted between the positive and negative electrodes. With the continuous development of lithium-ion battery technology, people have also put forward higher requirements on the performance of separators, especially in terms of heat resistance.

[0004] At present, the main means to improve the heat resistance of the diaphragm is to apply a heat-resistant coating on one or both sides of the diaphragm, and the most commonly used coating is a ceramic coating. Patent technology document CN202011334663.9 discloses a lithium-ion battery ceramic diaphragm and a preparation method thereof. Compared with the prior art, the lithium-ion battery ceramic diaphragm is thin and light and has excellent low thermal shrinkage and ion permeability. CN201510372721.X discloses a ceramic diaphragm for lithium-ion batteries and a lithium-ion battery. The ceramic diaphragm of the present invention avoids the introduction of highly toxic acrylonitrile monomers, making it safe and reliable during preparation and use, and reducing adverse effects on the environment and users. At the same time, the present invention is conducive to the preparation of a ceramic diaphragm with uniform distribution, good air permeability, and high bonding strength. However, when the lithium-ion battery is charged and discharged, the chemical reaction between the positive and negative electrodes will generate a certain amount of heat, and the resistance inside the battery will also cause the energy to be converted into heat energy. The heat will accumulate inside the battery and gradually increase the temperature of the battery, which will threaten the safety performance of the battery. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a ceramic diaphragm with stable safety and a preparation method thereof, so as to solve the problem of the lack of safety performance of traditional ceramic diaphragms.

[0006] Based on the above purpose, the present invention provides a ceramic composite diaphragm with stability and safety, comprising a ceramic diaphragm and a polymer coating on the surface of the ceramic diaphragm, wherein the polymer coating is obtained by coating a polymer coating liquid on the surface of the ceramic diaphragm, curing it in a coagulation bath, washing it with water, and drying it; the polymer coating liquid contains fluorinated aramid;

[0007] The preparation method of the fluorinated aramid is as follows: aramid is added into a sealed container, the air in the container is replaced with nitrogen, and then the temperature is raised to 100-110° C., a fluorine-nitrogen mixed gas is charged until the pressure in the container reaches 20-25 KPa, and then the container is allowed to stand for 30-40 minutes, the temperature is lowered, and alcohol washing is performed to obtain the fluorinated aramid;

[0008] Preferably, the volume ratio of fluorine gas to nitrogen gas in the fluorine-nitrogen mixed gas is 1:4.

[0009] Preferably, the polymer coating liquid comprises the following raw materials in parts by weight: 10-20 parts of fluorinated aramid, 0.3-5 parts of a binder, 0.1-1 parts of aluminum oxide, 60-95 parts of an organic solvent and 1-6 parts of deionized water.

[0010] Preferably, the binder is one or more of polyvinylidene fluoride-hexafluoropropylene, polyacrylonitrile, polyimide, and polymethyl methacrylate.

[0011] Preferably, the organic solvent is a mixture of one of DMAC, NMP, DMF, DMSO and 1-butyl-3-methylimidazolium tetrafluoroborate, with a weight ratio of 10:0.5-1.5.

[0012] Preferably, the particle size D50 of the aluminum oxide is 0.02-1 μm, and the bulk density is 0.8-1.8 g / m 2 .

[0013] Preferably, the ceramic diaphragm is obtained by coating ceramic slurry on both sides of a substrate and then drying;

[0014] Preferably, the ceramic slurry consists of ceramic particles, a binder, an additive and deionized water.

[0015] Preferably, the weight ratio of the ceramic particles, the binder, the additive and the deionized water is 20-50:1-5:0.01-0.1:50-80.

[0016] Preferably, the ceramic particles are one or more of alumina, boehmite, magnesium hydroxide, barium sulfate, lithium titanium aluminum phosphate, and aluminum nitride.

[0017] Preferably, the base film is one of a polypropylene base film, a polyethylene base film, a polymethylpentene base film, a non-woven fabric, and a polyimide base film.

[0018] Preferably, the binder is one or a mixture of polyacrylate, polyacrylate, polyacrylonitrile, and styrene-butadiene rubber.

[0019] Preferably, the auxiliary agent is one or a mixture of polyvinyl alcohol, sodium carboxymethyl cellulose, polymethyl methacrylate, acetylene glycol vinyl ether, and polyether-modified siloxanes.

[0020] Preferably, the polymer coating has a thickness of 0.5-4 μm and a bulk density of 0.8-1.8 g / m 2 .

[0021] Preferably, the melting point of the aramid is greater than 170°C.

[0022] Preferably, the coagulation bath is a mixture of one of DMAC, NMP, DMF, DMSO and deionized water, with a weight ratio of 1:4.

[0023] Furthermore, the present invention also provides a method for preparing a stable and safe ceramic composite diaphragm, the specific steps of which are as follows:

[0024] (1) Mixing an organic solvent and deionized water, then adding alumina, and stirring for 20-30 minutes to obtain a mixture;

[0025] (2) adding fluorinated aramid and a binder to the mixture, stirring for 50-60 minutes, and then filtering with a 250-mesh sieve to obtain a polymer coating liquid;

[0026] (3) The polymer coating liquid is applied to the surface of the ceramic diaphragm, which is then immersed in a coagulation bath, washed with water, and dried to obtain a ceramic composite diaphragm with stability and safety.

[0027] Beneficial effects of the present invention:

[0028] (1) The present invention uses fluorinated aramid as the raw material of the polymer coating liquid. Compared with directly using aramid as the raw material of the polymer coating liquid, the fluorinated aramid and the adhesive polyvinylidene fluoride-hexafluoropropylene and the organic solvent in the polymer coating liquid are more closely connected, thereby making the diaphragm obtained after the phase inversion of the polymer coating more compact, ultimately resulting in better adhesion and safety performance of the diaphragm.

[0029] (2) The present invention uses polyvinylidene fluoride-hexafluoropropylene as a binder for the polymer coating liquid, which can enhance the adhesion between the components in the polymer coating liquid, thereby making the polymer coating liquid more compact. At the same time, it also makes the components in the polymer coating liquid more evenly dispersed. The coating obtained after phase inversion is more compact, thereby making the adhesion performance and safety performance of the diaphragm better.

[0030] (3) The present invention mixes 1-butyl-3-methylimidazolium tetrafluoroborate with DMAC as an organic solvent, which can enhance the interfacial compatibility between the adhesive and the fluorinated aramid in the polymer coating liquid and the organic solvent, making the polymer coating liquid more uniform and compact. During the phase inversion process, the phase inversion process can be promoted, making the coating obtained after the phase inversion more compact, thereby making the adhesion of the diaphragm better and the safety performance better. DETAILED DESCRIPTION

[0031] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0032] The ceramic diaphragm used in the present invention is specifically prepared in the following steps:

[0033] (1) 35 g of aluminum oxide, 3 g of polyacrylate, 0.05 g of polymethyl methacrylate and 62 g of deionized water were mixed to obtain a ceramic slurry;

[0034] (2) uniformly coating the ceramic slurry on the upper and lower surfaces of the polypropylene base film and drying the same to obtain a ceramic diaphragm;

[0035] Example 1: A ceramic diaphragm with stability and safety, the specific preparation steps are as follows:

[0036] (1) 100 g of aramid is added into a sealed container, the air in the container is replaced with nitrogen, and then the temperature is raised to 100°C, and a fluorine-nitrogen mixed gas is introduced until the pressure in the container reaches 20 kPa, and then the container is allowed to stand for 30 minutes, cooled, and washed with alcohol to obtain fluorinated aramid, wherein the volume ratio of fluorine gas to nitrogen is 1:4.

[0037] (2) 60 g of DMAC and 1 g of deionized water were mixed, and then 0.1 g of aluminum oxide was added and stirred for 20 min to obtain a mixture. Subsequently, 10 g of fluorinated aramid and 0.3 g of polymethyl methacrylate were added to the mixture, stirred for 50 min, and then filtered with a 250-mesh sieve to obtain a polymer coating liquid;

[0038] (3) Mix DMAC and deionized water in a weight ratio of 1:4 and stir evenly to obtain a coagulation bath;

[0039] (4) The polymer coating liquid is coated on the upper and lower surfaces of the ceramic diaphragm by micro-gravure method, and then immersed in a coagulation bath, and then washed with water and dried to obtain a ceramic composite diaphragm with stability and safety.

[0040] Example 2: A ceramic diaphragm with stable safety, the specific preparation steps are as follows:

[0041] (1) 100 g of aramid was added into a sealed container, and the air in the container was replaced with nitrogen. The temperature was then raised to 105°C, and a fluorine-nitrogen mixed gas was introduced until the pressure in the container reached 23 kPa. The container was then allowed to stand for 35 minutes, cooled, and washed with alcohol to obtain fluorinated aramid, wherein the volume ratio of fluorine gas to nitrogen was 1:4.

[0042] (2) 80 g of DMF and 3 g of deionized water were mixed, and then 0.5 g of aluminum oxide was added and stirred for 25 min to obtain a mixture. Subsequently, 15 g of fluorinated aramid and 2.6 g of polyvinylidene fluoride-hexafluoropropylene were added to the mixture, stirred for 55 min, and then filtered with a 250-mesh sieve to obtain a polymer coating liquid;

[0043] (3) DMF and deionized water are mixed in a weight ratio of 1:4 and stirred evenly to obtain a coagulation bath;

[0044] (4) The polymer coating liquid is coated on the upper and lower surfaces of the ceramic diaphragm by micro-gravure method, and then immersed in a coagulation bath, and then washed with water and dried to obtain a ceramic composite diaphragm with stability and safety.

[0045] Example 3: A ceramic diaphragm with stable safety, the specific preparation steps are as follows:

[0046] (1) 100 g of aramid was added into a sealed container, and the air in the container was replaced with nitrogen. The temperature was then raised to 110°C, and a fluorine-nitrogen mixed gas was introduced until the pressure in the container reached 25 kPa. The container was then allowed to stand for 40 minutes, cooled, and washed with alcohol to obtain fluorinated aramid, wherein the volume ratio of fluorine gas to nitrogen was 1:4.

[0047] (2) 95 g of DMSO and 6 g of deionized water were mixed, and then 1 g of aluminum oxide was added and stirred for 30 min to obtain a mixture. Subsequently, 20 g of fluorinated aramid and 5 g of polyimide were added to the mixture, stirred for 60 min, and then filtered with a 250-mesh sieve to obtain a polymer coating liquid;

[0048] (3) Mix DMSO and deionized water in a weight ratio of 1:4 and stir evenly to obtain a coagulation bath;

[0049] (4) The polymer coating liquid is coated on the upper and lower surfaces of the ceramic diaphragm by micro-gravure method, and then immersed in a coagulation bath, and then washed with water and dried to obtain a ceramic composite diaphragm with stability and safety.

[0050] Example 4: A ceramic diaphragm with stability and safety, the specific preparation steps are as follows:

[0051] (1) 100 g of aramid was added into a sealed container, and the air in the container was replaced with nitrogen. The temperature was then raised to 105°C, and a fluorine-nitrogen mixed gas was introduced until the pressure in the container reached 23 kPa. The container was then allowed to stand for 35 minutes, cooled, and washed with alcohol to obtain fluorinated aramid, wherein the volume ratio of fluorine gas to nitrogen was 1:4.

[0052] (2) mixing 100 g of DMF with 5 g of 1-butyl-3-methylimidazolium tetrafluoroborate to obtain an organic solvent;

[0053] (3) 80 g of an organic solvent and 3 g of deionized water were mixed, and then 0.5 g of aluminum oxide was added and stirred for 25 min to obtain a mixture. Subsequently, 15 g of fluorinated aramid and 2.6 g of polyvinylidene fluoride-hexafluoropropylene were added to the mixture, stirred for 55 min, and then filtered with a 250-mesh sieve to obtain a polymer coating liquid;

[0054] (4) DMF and deionized water are mixed in a weight ratio of 1:4 and stirred evenly to obtain a coagulation bath;

[0055] (5) The polymer coating liquid is coated on the upper and lower surfaces of the ceramic diaphragm by micro-gravure method, and then immersed in a coagulation bath, and then washed with water and dried to obtain a ceramic composite diaphragm with stability and safety.

[0056] Example 5: A ceramic diaphragm with stable safety, the specific preparation steps are as follows:

[0057] (1) 100 g of aramid was added into a sealed container, and the air in the container was replaced with nitrogen. The temperature was then raised to 105°C, and a fluorine-nitrogen mixed gas was introduced until the pressure in the container reached 23 kPa. The container was then allowed to stand for 35 minutes, cooled, and washed with alcohol to obtain fluorinated aramid, wherein the volume ratio of fluorine gas to nitrogen was 1:4.

[0058] (2) mixing 100 g of DMF and 10 g of 1-butyl-3-methylimidazolium tetrafluoroborate to obtain an organic solvent;

[0059] (3) 80 g of an organic solvent and 3 g of deionized water were mixed, and then 0.5 g of aluminum oxide was added and stirred for 25 min to obtain a mixture. Subsequently, 15 g of fluorinated aramid and 2.6 g of polyvinylidene fluoride-hexafluoropropylene were added to the mixture, stirred for 55 min, and then filtered with a 250-mesh sieve to obtain a polymer coating liquid;

[0060] (4) DMF and deionized water are mixed in a weight ratio of 1:4 and stirred evenly to obtain a coagulation bath;

[0061] (5) The polymer coating liquid is coated on the upper and lower surfaces of the ceramic diaphragm by micro-gravure method, and then immersed in a coagulation bath, and then washed with water and dried to obtain a ceramic composite diaphragm with stability and safety.

[0062] Example 6: A ceramic diaphragm with stable safety, the specific preparation steps are as follows:

[0063] (1) 100 g of aramid was added into a sealed container, and the air in the container was replaced with nitrogen. The temperature was then raised to 105°C, and a fluorine-nitrogen mixed gas was introduced until the pressure in the container reached 23 kPa. The container was then allowed to stand for 35 minutes, cooled, and washed with alcohol to obtain fluorinated aramid, wherein the volume ratio of fluorine gas to nitrogen was 1:4.

[0064] (2) mixing 100 g of DMF with 15 g of 1-butyl-3-methylimidazolium tetrafluoroborate to obtain an organic solvent;

[0065] (3) 80 g of an organic solvent and 3 g of deionized water were mixed, and then 0.5 g of aluminum oxide was added and stirred for 25 min to obtain a mixture. Subsequently, 15 g of fluorinated aramid and 2.6 g of polyvinylidene fluoride-hexafluoropropylene were added to the mixture, stirred for 55 min, and then filtered with a 250-mesh sieve to obtain a polymer coating liquid;

[0066] (4) DMF and deionized water are mixed in a weight ratio of 1:4 and stirred evenly to obtain a coagulation bath;

[0067] (5) The polymer coating liquid is coated on the upper and lower surfaces of the ceramic diaphragm by micro-gravure method, and then immersed in a coagulation bath, and then washed with water and dried to obtain a ceramic composite diaphragm with stability and safety.

[0068] Example 7: A ceramic diaphragm with stable safety, the specific preparation steps are as follows:

[0069] (1) 100 g of aramid was added into a sealed container, and the air in the container was replaced with nitrogen. The temperature was then raised to 105°C, and a fluorine-nitrogen mixed gas was introduced until the pressure in the container reached 23 kPa. The container was then allowed to stand for 35 minutes, cooled, and washed with alcohol to obtain fluorinated aramid, wherein the volume ratio of fluorine gas to nitrogen was 1:4.

[0070] (2) mixing 100 g of DMF with 15 g of 1-butyl-3-methylimidazolium tetrafluoroborate to obtain an organic solvent;

[0071] (3) 80 g of an organic solvent and 3 g of deionized water were mixed, and then 0.5 g of aluminum oxide was added and stirred for 25 min to obtain a mixture. Subsequently, 15 g of fluorinated aramid and 2.6 g of polymethyl methacrylate were added to the mixture, stirred for 55 min, and then filtered with a 250-mesh sieve to obtain a polymer coating liquid;

[0072] (4) DMF and deionized water are mixed in a weight ratio of 1:4 and stirred evenly to obtain a coagulation bath;

[0073] (5) The polymer coating liquid is coated on the upper and lower surfaces of the ceramic diaphragm by micro-gravure method, and then immersed in a coagulation bath, and then washed with water and dried to obtain a ceramic composite diaphragm with stability and safety.

[0074] Comparative Example: A ceramic diaphragm with stable safety, the specific preparation steps are as follows:

[0075] (1) mixing 100 g of DMF and 10 g of 1-butyl-3-methylimidazolium tetrafluoroborate to obtain an organic solvent;

[0076] (2) 80 g of an organic solvent and 3 g of deionized water were mixed, and then 0.5 g of aluminum oxide was added and stirred for 25 min to obtain a mixture. Subsequently, 15 g of aramid fiber and 2.6 g of polyvinylidene fluoride-hexafluoropropylene were added to the mixture, stirred for 55 min, and then filtered with a 250-mesh sieve to obtain a polymer coating liquid;

[0077] (3) DMF and deionized water are mixed in a weight ratio of 1:4 and stirred evenly to obtain a coagulation bath;

[0078] (4) The polymer coating liquid is coated on the upper and lower surfaces of the ceramic diaphragm by micro-gravure method, and then immersed in a coagulation bath, and then washed with water and dried to obtain a ceramic composite diaphragm with stability and safety.

[0079] Performance Testing

[0080] Membrane breaking temperature:

[0081] The samples were tested using a Mettler thermomechanical analyzer with test parameters: heating from room temperature to 200°C, a heating rate of 5°C / min, and a load of 2g. The test results are shown in Table 1.

[0082]

[0083] It can be seen from Table 1 that, compared with the traditional ceramic diaphragm, after the polymer coating liquid is coated on its surface, its membrane rupture temperature is greatly increased, and in Example 5, when the polymer coating liquid contains fluorinated aramid, the adhesive is polyvinylidene fluoride-hexafluoropropylene, and the organic solvent contains 1-butyl-3-methylimidazole tetrafluoroborate, the membrane rupture temperature reaches the highest.

[0084] Adhesion test: The samples obtained in the embodiment and the comparative example were sandwiched between two PET films respectively; the temperature of the hot roller was tested with a temperature gun. After reaching the set temperature, the roller press switch was turned on, and the films were placed in parallel in the laminator. After all the films left the laminator, the PET films were peeled off, and the adhesion between the diaphragms was tested using a universal tensile machine. The test results are shown in Table 2.

[0085] Hot box test: 3 pieces of 100mm×100mm samples were uniformly cut from the samples obtained in the examples and comparative examples, and the sample lengths were accurately measured and the measuring points were marked. The samples were placed flat in a blast constant temperature oven that had reached the target temperature and was stable, with a layer of filter paper placed above and below the test samples. The samples were located in the middle of the drying oven, and after being placed under a constant temperature for the required time, they were taken out and the lengths between the longitudinal and transverse measuring points were measured. The longitudinal and transverse heat shrinkage rates were calculated according to the following formulas, and the values ​​of the 3 samples were taken and recorded. The test results are shown in Table 1.

[0086] ;

[0087] Wherein, S: shrinkage rate, %; L1: length before heating, mm; L2: length after heating, mm.

[0088] Hot needle puncture experiment:

[0089] The samples obtained in the embodiment and the comparative example were tested using a temperature-controlled soldering station (produced by Proskit) at a temperature of 400°C. The specific operation was as follows:

[0090] The samples obtained in the embodiment and the comparative example were tightened with circular tooling and fixed on a fixed position on the lifting platform. After the temperature of the equipment was raised to 400°C, the control knob of the hot needle (needle diameter 2 mm) was slowly turned downward. After the hot needle contacted the diaphragm, it stayed for 2 seconds, and then the knob was turned upward until the needle left the diaphragm. The diffusion diameter of the diaphragm after heating was measured with a steel ruler, and the relevant area was calculated. The test results are shown in Table 2.

[0091] Electrolyte high temperature immersion experiment:

[0092] (1) The samples obtained in the examples and comparative examples 1-3 were baked at 90°C for one hour, and immediately sealed in a sealed bag after being taken out. The test tubes were cleaned with alcohol (concentration ≥ 99%) and dried, and then sealed in a sealed bag. The diaphragm and the test tube were brought to a drying room, and the sealed bag was opened to allow the diaphragm and the test tube to stand in the drying room for 30 minutes;

[0093] (2) Place the samples after standing in a test tube, fill the test tube with electrolyte (choose new electrolyte that has not been used to ensure that the electrolyte does not absorb water), tighten the test tube and seal the test tube mouth with high temperature resistant tape;

[0094] (3) Mark the packaged samples and place them in an oven, baking them at 65°C for 7 days;

[0095] (4) Take out the sample and take a photo for preservation. After unsealing the test tube, seal the electrolyte and temporarily preserve it. Pour 200ml of alcohol (concentration ≥ 99%) into the beaker to clean the diaphragm. Flatten the diaphragm completely to ensure that it is completely cleaned. After cleaning, dry it with a hair dryer. When cleaning the next sample, pour out the used alcohol and pour in new alcohol for cleaning;

[0096] (5) The cleaned diaphragm was subjected to an adhesion test and a hot box test. The test results are shown in Table 2.

[0097]

[0098] Thermal runaway diffusion experiment:

[0099] (1) Take the battery cell or the smallest parallel unit at the center of the battery module as the thermal runaway trigger object, connect its positive and negative electrodes to the charging and discharging device and its voltage data sampling line, and maintain the electrical connection between the thermal runaway trigger object and the adjacent battery;

[0100] (2) Place the temperature sensors on the surface of all battery cells of the trigger object, equidistant from the positive and negative poles and closest to the positive and negative poles, set the temperature sampling period to 1s, and set the continuous monitoring of three temperature rise rate values ​​> 3℃ / s or fire or explosion as the judgment conditions for thermal runaway;

[0101] (3) Take the two battery cells adjacent to the triggering object as the thermal runaway monitoring objects, arrange the temperature sensor at the center position on the opposite side of the monitoring object surface adjacent to the triggering object or at the surface where the positive and negative poles of the monitoring object are located and equidistant from the positive and negative poles, use the ratio of the rated power of the triggering object to its nominal voltage as the current value to perform constant current charging on the triggering object, record the time, temperature and temperature rise rate of the triggering object, record the time, voltage, temperature and temperature rise rate of the monitoring object, and observe the battery cell status.

[0102] (4) Disconnect the test sample from the charging and discharging device, remove the data sampling line, and take out the test sample;

[0103] (5) Determine whether thermal runaway occurs in the monitored object based on the thermal runaway determination conditions, and record the time, temperature, and cell status when thermal runaway spreads. The test results are shown in Table 3.

[0104]

[0105] Data analysis: From Tables 2 and 3, it can be seen from Examples 2 and 1 and 3 that when the binder in the polymer coating liquid is polyvinylidene fluoride-hexafluoropropylene, the compatibility of polyvinylidene fluoride-hexafluoropropylene with fluorinated aramid is better, and thus the obtained diaphragm has better adhesion and better safety performance, and this conclusion is confirmed again from Examples 5 and 7;

[0106] It can be seen from Examples 2 and 5 that when the organic solvent in the polymer coating liquid contains 1-butyl-3-methylimidazolium tetrafluoroborate, the phase inversion process can be promoted during the phase inversion, and at the same time, the polymer coating liquid can have a better interface compatibility with polyvinylidene fluoride-hexafluoropropylene and fluorinated aramid, thereby making the adhesion of the diaphragm better and the safety performance better.

[0107] It can be seen from Example 5 and the comparative example that, compared with the diaphragm obtained by directly using aramid as the raw material of the polymer coating liquid in the prior art, the diaphragm obtained by using fluorinated aramid as the raw material of the polymer coating liquid is more excellent in both adhesion performance and safety performance.

[0108] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

[0109] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A ceramic composite diaphragm with stability and safety, characterized in that: It includes a ceramic diaphragm and a polymer coating on the surface of the ceramic diaphragm, wherein the polymer coating is obtained by coating a polymer coating liquid on the surface of the ceramic diaphragm, curing it in a coagulation bath, washing it with water, and drying it; the polymer coating liquid contains fluorinated aramid; The preparation method of the fluorinated aramid is as follows: aramid is added into a sealed container, the air in the container is replaced with nitrogen, and then the temperature is raised to 100-110° C., a fluorine-nitrogen mixed gas is charged until the pressure in the container reaches 20-25 KPa, and then the container is allowed to stand for 30-40 minutes, the temperature is lowered, and alcohol washing is performed to obtain the fluorinated aramid; The volume ratio of fluorine gas to nitrogen in the fluorine-nitrogen mixed gas is 1:4; The polymer coating liquid comprises the following raw materials in parts by weight: 10-20 parts of fluorinated aramid, 0.3-5 parts of a binder, 0.1-1 parts of aluminum oxide, 60-95 parts of an organic solvent and 1-6 parts of deionized water; The binder is polyvinylidene fluoride-hexafluoropropylene; The organic solvent is a mixture of one of DMAC, NMP, DMF, and DMSO and 1-butyl-3-methylimidazole tetrafluoroborate, with a weight ratio of 10:0.5-1.

5.

2. The stable and safe ceramic composite diaphragm according to claim 1, characterized in that: The particle size D50 of the aluminum oxide is 0.02-1 μm.

3. The stable and safe ceramic composite diaphragm according to claim 1, characterized in that: The ceramic diaphragm is obtained by coating ceramic slurry on both sides of a substrate and then drying the substrate; the ceramic slurry is composed of ceramic particles, a binder, an additive and deionized water.

4. The stable and safe ceramic composite diaphragm according to claim 1, characterized in that: The polymer coating has a thickness of 0.5-4 μm and a bulk density of 0.8-1.8 g / m 2 .

5. The stable and safe ceramic composite diaphragm according to claim 1, characterized in that: The melting point of the aramid fiber is greater than 170°C.

6. The stable and safe ceramic composite diaphragm according to claim 1, characterized in that: The coagulation bath is a mixture of one of DMAC, NMP, DMF, DMSO and deionized water, with a weight ratio of 1:

4.

7. A method for preparing a stable and safe ceramic composite diaphragm according to any one of claims 1 to 6, characterized in that: The specific preparation steps are as follows: (1) Mixing an organic solvent and deionized water, then adding alumina, and stirring for 20-30 minutes to obtain a mixture; (2) adding fluorinated aramid and a binder to the mixture, stirring for 50-60 minutes, and then filtering with a 250-mesh sieve to obtain a polymer coating liquid; (3) The polymer coating liquid is applied to the surface of the ceramic diaphragm, which is then immersed in a coagulation bath, washed with water, and dried to obtain a ceramic composite diaphragm with stability and safety.

Citation Information

Patent Citations

  • Ceramic separators for lithium-ion batteries and lithium-ion batteries

    CN106328869B

  • Lithium ion battery ceramic diaphragm and preparation method thereof

    CN112467307A

  • Aramid III fiber with fluorine-containing surface and preparation method thereof

    CN101798748A

  • Polymer coating separator and preparation method thereof

    CN107240663A

  • Colored ceramic coating film coated with aramid polymer, and preparation method thereof

    CN108711603A