Aluminum-based composite material with high elastic modulus and high thermal conductivity and preparation method thereof

By preparing three-dimensional graphene/MgAl2O4 composite materials, the problems of low elastic modulus and thermal conductivity of aluminum alloy mid-plate and battery protection board materials were solved, realizing the preparation of high-performance and low-cost aluminum-based composite materials, which are suitable for mid-plate and battery protection boards of 3C products such as mobile phones and tablets.

CN118460873BActive Publication Date: 2024-11-19广州众山功能材料有限公司 +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410910035.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-19
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

Existing aluminum alloy middle plates and battery protection plate materials have problems such as low elastic modulus and low thermal conductivity. Furthermore, existing preparation methods have defects such as difficulty in forming, uneven distribution of reinforcing phase, safety hazards, and difficulty in high-temperature control.

Method used

A three-dimensional graphene/MgAl2O4 composite material was synthesized by a solvothermal method. Combined with cold isostatic pressing and vacuum hot pressing processes, an aluminum-based composite material with high elastic modulus and high thermal conductivity was prepared, avoiding high-temperature treatment and expensive equipment.

Benefits of technology

This study achieved high thermal conductivity and high elastic modulus in aluminum-based composite materials, ensuring the plastic processing performance of the materials, reducing production costs, and improving the dispersibility and interfacial bonding of the materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118460873B_ABST
    Figure CN118460873B_ABST
Patent Text Reader

Abstract

The invention relates to an aluminum-based composite material with high elastic modulus and high thermal conductivity and a preparation method thereof. In the preparation process of the composite material, isopropyl alcohol is used as a solvent, diethanolamine is added during the reaction process, three-dimensional graphene / nano-wire-shaped MgAl2O4 is innovatively synthesized for the first time, and the three-dimensional graphene / nano-wire-shaped MgAl2O4 is used as a reinforcing phase. The aluminum-based composite material is prepared by cold isostatic pressing and vacuum hot pressing. The three-dimensional graphene / nano-wire-shaped MgAl2O4 work synergistically to effectively improve the elastic modulus and thermal conductivity of the aluminum-based composite material, thereby ensuring that subsequent plastic processing, such as forging, rolling and stamping, can be carried out smoothly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an aluminum-based composite material with high elastic modulus and high thermal conductivity, a preparation method thereof and applications thereof. Background Art

[0002] 3C products, especially the middle plates and battery protection plates of mobile phones and tablets, are currently mainly made of aluminum alloy. Aluminum alloy has good heat dissipation performance and its specific modulus is better than that of stainless steel and copper alloy. Therefore, the use of aluminum alloy to prepare middle plates has a good cost-effectiveness. However, the absolute modulus of aluminum alloy is low and the thermal conductivity is lower than that of copper alloy. Therefore, a material with high elastic modulus and high thermal conductivity is the best choice for middle plates and battery protection plates.

[0003] Graphene is a two-dimensional planar nanomaterial with high electrical conductivity, high thermal conductivity, high modulus and high strength. Its excellent mechanical and physical properties enable it to have a wide range of high-end applications. It is an ideal structural heat dissipation material with extremely high market potential value.

[0004] A Chinese invention patent with publication number CN106591666B discloses a graphene-reinforced aluminum-based silicon carbide composite material, a preparation method thereof, and an application thereof. The silicon carbide content thereof is 40% to 70%. The high volume fraction of particles leads to difficulty in molding. The volume fraction of the added silicon carbide reinforcement phase is too high, and the elongation of the aluminum-based composite material is greatly reduced, which is very unfavorable for the back-end stamping molding and is more difficult for the processing and molding of thin plates.

[0005] The Chinese invention patent with the publication number CN108950280B discloses a graphene / silicon carbide reinforced aluminum-based composite material and a preparation method thereof, wherein the graphene-coated silicon carbide composite material is uniformly distributed in a metal Al matrix, and the silicon carbide is first coated with graphene. In this process, it is not necessary to prepare graphene separately first, but to wet-mill the graphite flakes and silicon carbide nanoparticles to directly obtain the silicon carbide particles coated with graphene, and the entire preparation process is completed in one step; and then the silicon carbide coated with graphene is used as a reinforcing phase and sintered and composited with metal aluminum in a certain proportion to improve the strength, density, electrical conductivity and mechanical properties of the metal aluminum. However, the reinforcing phase material agglomerates seriously, which greatly affects the thermal conductivity and density of the aluminum-based composite material.

[0006] The Chinese invention patent with the publication number CN105801154A discloses a graphene-enhanced aluminum-based silicon carbide composite material and a preparation method thereof. The composite material uses graphite oxide as a carbon source, and a layer of SiO2 particles is wrapped on the surface of the reduced graphene oxide by a hydrothermal method, so that the graphene and SiC form a good interface layer and are evenly dispersed; after high-temperature sintering, a carbon thermal reduction reaction is performed at the interface between graphene and SiO2, and silicon carbide whiskers and particles are grown in situ, the interface strength and oxidation resistance are improved, the interface strengthening effect is generated, the crack propagation resistance is increased, and the fracture toughness of the ceramic is further improved, so as to overcome the defects of poor graphene dispersibility and poor high-temperature oxidation resistance in the preparation technology of graphene / silicon carbide composite materials, and the in-situ growth, crack self-healing and toughening mechanism are applied to the preparation technology of graphene / silicon carbide materials, thereby obtaining graphene-toughened silicon carbide ceramics with excellent mechanical properties and interface bonding properties. However, this method requires high-temperature sintering and carbon thermal reduction reaction, and there is a defect that the reaction process is difficult to control.

[0007] The Chinese invention patent with publication number CN104264000A discloses a method for preparing graphene-enhanced aluminum-based silicon carbide composite materials by powder metallurgy, comprising the following steps: 1) soaking the reinforcement particles in a strong acid solution, then washing with deionized water until neutral, removing surface impurities, and drying to obtain activated reinforcement particles; 2) adding the activated reinforcement particles to the graphene dispersion, coating the surface with graphene nanosheets by mechanical stirring or ultrasonic dispersion, and obtaining graphene-modified reinforcement particles; 3) mixing the graphene-modified reinforcement particles with aluminum matrix powder, and obtaining graphene-modified high thermal conductivity aluminum-based composite materials by pressing and sintering. The composite material obtained by this method has a glossy surface, isotropic, has few pore defects, is easy to change the volume fraction of the reinforcement phase, and is easy to regulate the performance of the composite material. However, strong acid is required, which has safety hazards, many wastes and is not conducive to environmental protection.

[0008] The Chinese invention patent with publication number CN104848748A discloses a method for preparing graphene-enhanced aluminum silicon carbide composite materials by pressure infiltration, wherein the method mixes graphene with an ethanol solution to obtain a uniformly dispersed graphene ethanol dispersion, then adds SiC powder to the graphene ethanol dispersion, ball mills, mixes evenly, dries, presses the mixture into a skeleton, and adds high-temperature aluminum liquid to the skeleton by pressure infiltration to obtain a graphene-enhanced aluminum silicon carbide composite material. This method has the advantages of simple forming and no need for subsequent complex mechanical processing, but there are problems such as uneven distribution of the reinforcement phase and pore defects, which leads to defects such as anisotropy of material properties, large surface, inability to control the amount of silicon carbide volume addition and other reinforcement phase (such as graphene) content. In addition, the method prepares the graphene / silicon carbide reinforced aluminum-based composite material by preparing a SiC ceramic preform under pressure infiltration, which requires heating the aluminum liquid to 700-750°C, resulting in control difficulties and safety issues; and the graphene ethanol dispersion is added to the aluminum silicon carbide composite material by ball milling (about 10-20 hours), which has defects such as uneven mixing. Summary of the invention

[0009] In order to solve the above problems, the present invention provides a high thermal conductivity aluminum-based composite material and a preparation method, while improving the elastic modulus and elongation. In addition, the production process is simple and does not require expensive production equipment. The aluminum-based composite material prepared by this method has the characteristics of high performance and low cost.

[0010] In order to achieve the above object, the present invention adopts the following technical scheme:

[0011] A method for preparing an aluminum-based composite material with high elastic modulus and high thermal conductivity comprises the following steps:

[0012] Step (1): weighing graphene oxide, aluminum source and magnesium source in proportion, dissolving them in isopropanol, and performing ultrasonic treatment;

[0013] Step (2): adding diethanolamine to the above precursor solution and stirring;

[0014] Step (3): placing the solution of step (2) in a high pressure reactor and reacting at 180-210° C. for 15-18 hours; after the reaction, washing and freeze drying to obtain three-dimensional graphene / MgAl2O4;

[0015] Step (4): batching, according to the mass ratio, weigh 10%-25% of three-dimensional graphene / MgAl2O4, 0.5%-1.5% of Cu, 1%-2% of Mg, 0.3%-1% of Si, and the rest of Al; mix Cu, Mg, Si, Al and ethanol and perform high-energy ball milling, wherein the high-energy ball milling process is to perform ball milling at a speed of 280-320 r / min for 8-10 hours; then, add the three-dimensional graphene / MgAl2O4 and perform low-energy ball milling at a speed of 180-200 r / min for 3-9 hours; after the ball milling is completed, vacuum drying is performed;

[0016] Step (5): cold isostatic pressing, the dried powder is loaded into a mold, sealed, and then put into a cold isostatic press for pressing and then demolding;

[0017] Step (6): Vacuum hot pressing. The green body after cold isostatic pressing is put into a vacuum hot pressing furnace for hot pressing and sintering.

[0018] The median particle size of Al, Cu, Mg and Si is 2 to 30 μm;

[0019] The amount of ethanol added is 1-2 times the weight of the ball-milled powder;

[0020] In step (4), the mass ratio of the ball mill powder to the ball material is 1:10-1:20; the protective atmosphere is argon;

[0021] The vacuum degree of the vacuum drying in step (4) is 0.1-0.5 Pa, and the drying temperature is 60-100°C.

[0022] Furthermore, the cold isostatic pressing pressure in step (5) is 150-300 MPa, and the holding time is 10-30 min;

[0023] Furthermore, the vacuum hot pressing in step (6) comprises the following steps:

[0024] 1) 20-40℃, evacuate for 1-3 hours, and the vacuum degree reaches 0.01-0.05Pa;

[0025] 2) Heating to 300-500°C and pressurizing to 60-120MPa;

[0026] 3) Raise the temperature to 400-600℃ and keep the temperature and pressure for 1-2 hours;

[0027] 4) Cool to room temperature and take out the green body;

[0028] The beneficial effects of the present invention are:

[0029] (1) The present invention uses isopropanol as solvent and adds a certain amount of diethanolamine to synthesize three-dimensional graphene / nanowire MgAl2O4 for the first time in an innovative way. The two-dimensional graphene sheets overlap each other to form a three-dimensional thermal conductive network structure. Compared with ordinary graphene, it has higher mechanical strength, impact damage resistance and crack propagation resistance. MgAl2O4 has a similar crystal structure to aluminum and has many advantages such as high melting point, high modulus, high strength and low expansion coefficient. The three-dimensional graphene can make the MgAl2O4 nanowire overlap on the stone. On the graphene sheets, the agglomeration of MgAl2O4 nanowires is effectively avoided, making the Orowan strengthening effect more prominent; and the MgAl2O4 nanowires are introduced between the graphene sheets to form a barrier effect on the two-dimensional graphene sheets, further improving the dispersion of the graphene sheets and avoiding the collapse of the three-dimensional structure, thereby increasing its contact area with the aluminum material; a multi-level three-dimensional structure is formed through one-dimensional wire-two-dimensional surface, which is beneficial to the transmission of stress during deformation, ensures the mechanical properties of the material, and can achieve the technical effects of synergistic toughening and thermal conductivity.

[0030] (2) This application improves the thermal conductivity of aluminum-based composite materials by introducing three-dimensional graphene / MgAl2O4. Only a small amount of three-dimensional graphene / MgAl2O4 (less than 30% added) is needed to increase the elongation of aluminum-based composite materials (greater than 5%), thereby ensuring that subsequent plastic processing, such as forging, rolling and stamping, can proceed smoothly. Secondly, the method of cold isostatic pressing plus vacuum hot pressing has lower cost and higher efficiency than traditional hot isostatic pressing.

[0031] (3) The present application adjusts the ball milling process, firstly ball mills Cu, Mg, Si and Al at high speed, then adds three-dimensional graphene / MgAl2O4 for low-speed ball milling after the ball milling, and optimizes the ball milling parameters to ensure the miscibility while avoiding the damage of the three-dimensional graphene / MgAl2O4 structure.

[0032] (4) The three-dimensional graphene obtained in the present application has not undergone a high-temperature heat treatment process. While ensuring thermal conductivity, a small amount of functional groups are retained on its surface, which improves its dispersion performance and maintains good wettability and interface bonding with the aluminum matrix.

[0033] (5) The preparation process is simple, no high temperature treatment is required, and no expensive production equipment is required. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Attached Figure 1 This is a scanning electron microscope image of the three-dimensional graphene prepared by solvothermal method in this application;

[0035] Attached Figure 2 This is a scanning electron microscope image of the three-dimensional graphene / MgAl2O4 of Example 1. DETAILED DESCRIPTION

[0036] Example 1, step (1): 800 mg of graphene oxide, 0.04 mol of aluminum nitrate and 0.02 mol of magnesium nitrate were weighed, dissolved in 100 ml of isopropanol, and subjected to ultrasonic treatment;

[0037] Step (2): Add 18 mg of diethanolamine to the above precursor solution and stir;

[0038] Step (3): placing the solution of step (2) in a high pressure reactor and reacting at 200°C for 15 hours; after the reaction is completed, washing and freeze drying;

[0039] Step (4): batching, according to the mass ratio, weigh 15% of three-dimensional graphene / MgAl2O4, 1.5% of Cu, 1% of Mg, 1% of Si, and the rest of Al; mix Cu, Mg, Si, Al with ethanol and perform high-energy ball milling, wherein the high-energy ball milling process is to perform ball milling at a speed of 310 r / min for 10 h; then, add the three-dimensional graphene / MgAl2O4 and perform ball milling at a speed of 180 r / min for 4 h; after the ball milling is completed, vacuum drying is performed;

[0040] Step (5): cold isostatic pressing: the dried powder is loaded into a mold, sealed and then pressed into a cold isostatic press at a pressing pressure of 200 MPa for 10 min. After the pressing is completed, the powder is demoulded;

[0041] Step (6): Vacuum hot pressing. After cold isostatic pressing, the green body is put into a vacuum hot pressing furnace for hot pressing and sintering. The vacuum degree reaches 4.0×10 -2 Pa, and began to heat up. When the temperature reached 300°C, pressure was applied at 70MPa. After pressurization, the temperature continued to rise to 560°C, and the temperature and pressure were maintained for 1 hour to obtain a three-dimensional graphene / MgAl2O4 aluminum-based composite material.

[0042] Example 2, step (1): weigh 900 mg of graphene oxide, 0.04 mol of aluminum nitrate and 0.02 mol of magnesium nitrate, dissolve in 100 ml of isopropanol, and treat with ultrasound;

[0043] Step (2): Add 22 mg of diethanolamine to the above precursor solution and stir;

[0044] Step (3): placing the solution of step (2) in a high pressure reactor and reacting at 200°C for 15 hours; after the reaction is completed, washing and freeze drying;

[0045] Step (4): batching, according to the mass ratio, weigh 15% of three-dimensional graphene / MgAl2O4, 1.5% of Cu, 1% of Mg, 1% of Si, and the rest of Al; mix Cu, Mg, Si, Al with ethanol and perform high-energy ball milling, wherein the high-energy ball milling process is to perform ball milling at a speed of 310 r / min for 10 h; then, add the three-dimensional graphene / MgAl2O4 and perform ball milling at a speed of 180 r / min for 4 h; after the ball milling is completed, vacuum drying is performed;

[0046] Step (5): cold isostatic pressing: the dried powder is loaded into a mold, sealed and then pressed into a cold isostatic press at a pressing pressure of 200 MPa for 10 min. After the pressing is completed, the powder is demoulded;

[0047] Step (6): Vacuum hot pressing. After cold isostatic pressing, the green body is put into a vacuum hot pressing furnace for hot pressing and sintering. The vacuum degree reaches 4.0×10 -2 Pa, and began to heat up. When the temperature reached 300°C, pressure was applied at 70MPa. After pressurization, the temperature continued to rise to 560°C, and the temperature and pressure were maintained for 1 hour to obtain a three-dimensional graphene / MgAl2O4 aluminum-based composite material.

[0048] Example 3, step (1): weigh 800 mg of graphene oxide, 0.04 mol of aluminum nitrate and 0.02 mol of magnesium nitrate, dissolve in 100 ml of isopropanol, and treat with ultrasound;

[0049] Step (2): Add 22 mg of diethanolamine to the above precursor solution and stir;

[0050] Step (3): placing the solution of step (2) in a high pressure reactor and reacting at 210° C. for 15 h; after the reaction is completed, washing and freeze drying;

[0051] Step (4): batching, according to the mass ratio, weigh 15% of three-dimensional graphene / MgAl2O4, 1.5% of Cu, 1% of Mg, 1% of Si, and the rest of Al; mix Cu, Mg, Si, Al with ethanol and perform high-energy ball milling, wherein the high-energy ball milling process is to perform ball milling at a speed of 310 r / min for 10 h; then, add three-dimensional graphene / MgAl2O4 and perform ball milling at a speed of 180 r / min for 5 h; after the ball milling is completed, vacuum drying is performed;

[0052] Step (5): cold isostatic pressing: the dried powder is loaded into a mold, sealed and then pressed into a cold isostatic press at a pressing pressure of 200 MPa for 10 min. After the pressing is completed, the powder is demoulded;

[0053] Step (6): Vacuum hot pressing. After cold isostatic pressing, the green body is put into a vacuum hot pressing furnace for hot pressing and sintering. The vacuum degree reaches 4.0×10-2 Pa, and began to heat up. When the temperature reached 300°C, pressure was applied at 70MPa. After pressurization, the temperature continued to rise to 560°C, and the temperature and pressure were maintained for 1 hour to obtain a three-dimensional graphene / MgAl2O4 aluminum-based composite material.

[0054] Example 4, step (1): 800 mg of graphene oxide, 0.04 mol of aluminum nitrate and 0.02 mol of magnesium nitrate were weighed, dissolved in 100 ml of isopropanol, and subjected to ultrasonic treatment;

[0055] Step (2): Add 18 mg of diethanolamine to the above precursor solution and stir;

[0056] Step (3): placing the solution of step (2) in a high pressure reactor and reacting at 200°C for 15 hours; after the reaction is completed, washing and freeze drying;

[0057] Step (4): batching, according to the mass ratio, weigh 20% of three-dimensional graphene / MgAl2O4, 1.5% of Cu, 1% of Mg, 1% of Si, and the rest of Al; mix Cu, Mg, Si, Al with ethanol and perform high-energy ball milling, wherein the high-energy ball milling process is to perform ball milling at a speed of 310 r / min for 10 h; then, add the three-dimensional graphene / MgAl2O4 and perform ball milling at a speed of 180 r / min for 4 h; after the ball milling is completed, vacuum drying is performed;

[0058] Step (5): cold isostatic pressing: the dried powder is loaded into a mold, sealed and then pressed into a cold isostatic press at a pressing pressure of 200 MPa for 10 min. After the pressing is completed, the powder is demoulded;

[0059] Step (6): Vacuum hot pressing. After cold isostatic pressing, the green body is put into a vacuum hot pressing furnace for hot pressing and sintering. The vacuum degree reaches 4.0×10 -2 Pa, and began to heat up. When the temperature reached 300°C, pressure was applied at 70MPa. After pressurization, the temperature continued to rise to 560°C, and the temperature and pressure were maintained for 1 hour to obtain a three-dimensional graphene / MgAl2O4 aluminum-based composite material.

[0060] Comparative Example 1, step (1): weigh 0.04 mol aluminum nitrate and 0.02 mol magnesium nitrate, dissolve in 100 ml isopropanol, and treat with ultrasound;

[0061] Step (2): Add 18 mg of diethanolamine to the above precursor solution and stir;

[0062] Step (3): placing the precursor solution of step (2) in a high pressure reactor and reacting at 200°C for 15 hours; after the reaction is completed, washing and freeze drying;

[0063] Step (4): batching, using thermogravimetric TG to measure the ratio of graphene to MgAl2O4 in Example 1 (about 0.12); according to the mass ratio obtained by the test, weigh commercially available ordinary graphene, according to (graphene + MgAl2O4) 15%, Cu 1.5%, Mg 1%, Si 1%, and the rest Al; mix Cu, Mg, Si, Al with ethanol and perform high-energy ball milling, wherein the high-energy ball milling process is to ball mill at a speed of 310 r / min for 10 h; then, add (graphene + MgAl2O4) and ball mill at a speed of 180 r / min for 4 h; after the ball milling is completed, vacuum drying;

[0064] Step (5): cold isostatic pressing: the dried powder is loaded into a mold, sealed and then pressed into a cold isostatic press at a pressing pressure of 200 MPa for 10 min. After the pressing is completed, the powder is demoulded;

[0065] Step (6): Vacuum hot pressing. After cold isostatic pressing, the green body is put into a vacuum hot pressing furnace for hot pressing and sintering. The vacuum degree reaches 4.0×10 -2 Pa, and began to heat up. When the temperature reached 300°C, pressure was applied at 70MPa. After pressurization, the temperature continued to rise to 560°C, and the temperature and pressure were maintained for 1 hour to obtain a two-dimensional graphene sheet + MgAl2O4 aluminum-based composite material.

[0066] Comparative Example 2, step (1): 800 mg of graphene oxide was weighed and dissolved in 100 ml of isopropanol. After ultrasonic treatment, the solution was placed in a high-pressure reactor and reacted at 200° C. for 15 h. After the reaction was completed, the mixture was washed and freeze-dried;

[0067] Step (2): weigh 0.04 mol aluminum nitrate and 0.02 mol magnesium nitrate, dissolve them in 100 ml isopropanol, and treat with ultrasound;

[0068] Add 18 mg of diethanolamine to the above precursor solution and stir;

[0069] Step (3) the precursor solution is placed in a high pressure reactor and reacted at 200°C for 15 hours; after the reaction is completed, the precursor solution is washed and freeze-dried;

[0070] Step (4): batching, according to the mass ratio, weigh 15% of the graphene in step (1) and the MgAl2O4 mixture in step (3), 1.5% of Cu, 1% of Mg, 1% of Si, and the rest of Al; mix Cu, Mg, Si, Al with ethanol and perform high-energy ball milling, wherein the high-energy ball milling process is to perform ball milling at a speed of 310 r / min for 10 h; then, add graphene / MgAl2O4 and perform ball milling at a speed of 180 r / min for 4 h; after the ball milling is completed, vacuum drying is performed;

[0071] Step (5): cold isostatic pressing: the dried powder is loaded into a mold, sealed and then pressed into a cold isostatic press at a pressing pressure of 200 MPa for 10 min. After the pressing is completed, the powder is demoulded;

[0072] Step (6): Vacuum hot pressing. After cold isostatic pressing, the green body is put into a vacuum hot pressing furnace for hot pressing and sintering. The vacuum degree reaches 4.0×10 -2 Pa, and then the temperature was raised to 300 ° C. The pressure was 70 MPa. After the pressure was raised, the temperature was raised to 560 ° C. The temperature was kept at this temperature for 1 hour to obtain a three-dimensional graphene + MgAl2O4 mixed reinforced aluminum matrix composite material.

[0073] Comparative Example 3, step (1): weigh 800 mg of graphene oxide, 0.04 mol of aluminum nitrate and 0.02 mol of magnesium nitrate, dissolve in 100 ml of isopropanol, and treat with ultrasound;

[0074] Step (2): Add 18 mg of diethanolamine to the above precursor solution and stir;

[0075] Step (3): placing the precursor solution of step (2) in a high pressure reactor and reacting at 200°C for 15 hours; after the reaction is completed, washing and freeze drying;

[0076] Step (4): batching, weighing 15% of three-dimensional graphene / MgAl2O4, 1.5% of Cu, 1% of Mg, 1% of Si, and the rest of Al according to the mass ratio; mixing Cu, Mg, Si, Al, graphene / MgAl2O4 with ethanol and ball milling, wherein the high-energy ball milling process is ball milling at a speed of 310 r / min for 14 h; after the ball milling is completed, vacuum drying is performed;

[0077] Step (5): cold isostatic pressing: the dried powder is loaded into a mold, sealed and then pressed into a cold isostatic press at a pressing pressure of 200 MPa for 10 min. After the pressing is completed, the powder is demoulded;

[0078] Step (6): Vacuum hot pressing. After cold isostatic pressing, the green body is put into a vacuum hot pressing furnace for hot pressing and sintering. The vacuum degree reaches 4.0×10 -2 Pa, and then the temperature began to rise. When the temperature reached 300°C, the pressure began to increase, and the pressure was 70MPa. After the pressure was increased, the temperature continued to rise to 560°C, and the temperature and pressure were kept for 1 hour to obtain an aluminum-based material reinforced with a three-dimensional graphene / MgAl2O4 aluminum-based composite material.

[0079] Comparative Example 4, step (1): weigh 800 mg of graphene oxide, 0.04 mol of aluminum nitrate and 0.02 mol of magnesium nitrate, dissolve in 100 ml of water, and perform ultrasonic treatment;

[0080] Step (2): Add 18 mg of diethanolamine to the above precursor solution and stir;

[0081] Step (3): placing the solution of step (2) in a high pressure reactor and reacting at 200°C for 15 hours; after the reaction is completed, washing and freeze drying;

[0082] Step (4): batching, according to the mass ratio, weigh 15% of three-dimensional graphene / MgAl2O4, 1.5% of Cu, 1% of Mg, 1% of Si, and the rest of Al; mix Cu, Mg, Si, Al with ethanol and perform high-energy ball milling, wherein the high-energy ball milling process is to perform ball milling at a speed of 310 r / min for 10 h; then, add the three-dimensional graphene / MgAl2O4 and perform ball milling at a speed of 180 r / min for 4 h; after the ball milling is completed, vacuum drying is performed;

[0083] Step (5): cold isostatic pressing: the dried powder is loaded into a mold, sealed and then pressed into a cold isostatic press at a pressing pressure of 200 MPa for 10 min. After the pressing is completed, the powder is demoulded;

[0084] Step (6): Vacuum hot pressing. After cold isostatic pressing, the green body is put into a vacuum hot pressing furnace for hot pressing and sintering. The vacuum degree reaches 4.0×10 -2 Pa, and began to heat up. When the temperature reached 300°C, pressure was applied at 70MPa. After pressurization, the temperature continued to rise to 560°C, and the temperature and pressure were maintained for 1 hour to obtain a three-dimensional graphene / MgAl2O4 aluminum-based composite material.

[0085] Comparative Example 5, step (1): 800 mg of graphene oxide, 0.04 mol of aluminum nitrate and 0.02 mol of magnesium nitrate were weighed, dissolved in 100 ml of isopropanol, and subjected to ultrasonic treatment;

[0086] Step (2): placing the solution of step (1) in a high pressure reactor and reacting at 200° C. for 15 h; after the reaction is completed, washing and freeze drying;

[0087] Step (3): batching, according to the mass ratio, weigh 15% of three-dimensional graphene / MgAl2O4, 1.5% of Cu, 1% of Mg, 1% of Si, and the rest of Al; mix Cu, Mg, Si, Al with ethanol and perform high-energy ball milling, wherein the high-energy ball milling process is to perform ball milling at a speed of 310 r / min for 10 h; then, add three-dimensional graphene / MgAl2O4 and perform ball milling at a speed of 180 r / min for 4 h; after the ball milling is completed, vacuum drying is performed;

[0088] Step (4): cold isostatic pressing: the dried powder is loaded into a mold, sealed and then pressed into a cold isostatic press at a pressing pressure of 200 MPa for 10 min. After the pressing is completed, the powder is demoulded;

[0089] Step (5): Vacuum hot pressing. After cold isostatic pressing, the green body is put into a vacuum hot pressing furnace for hot pressing and sintering. The vacuum degree reaches 4.0×10 -2 Pa, and began to heat up. When the temperature reached 300°C, pressure was applied at 70MPa. After pressurization, the temperature continued to rise to 560°C, and the temperature and pressure were maintained for 1 hour to obtain a three-dimensional graphene / MgAl2O4 aluminum-based composite material.

[0090] The thermal conductivity, elastic modulus and elongation of the materials of Examples 1-4 and Comparative Examples 1-5 were tested, and the results are shown in the following table:

[0091] Table 1: Test data of thermal conductivity, elastic modulus and elongation of materials of Examples 1-4 and Comparative Examples 1-5

[0092]

[0093] It can be seen from Examples 1-4 and Comparative Examples 1-5 and Table 1 that the present invention has good thermal conductivity and elasticity, and can meet the functional requirements of 3C products such as mobile phone back panels.

[0094] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A method for preparing an aluminum-based composite material with high elastic modulus and high thermal conductivity, characterized in that: The steps include: Step (1): weighing graphene oxide, an aluminum source and a magnesium source in proportion, dissolving them in isopropanol, and ultrasonically treating them to obtain a precursor solution; Step (2): adding diethanolamine to the above precursor solution and stirring; Step (3): placing the solution of step (2) in a high pressure reactor and reacting at 180-210° C. for 15-18 hours; after the reaction, washing and freeze drying are performed to obtain three-dimensional graphene / MgAl2O4; Step (4): batching, weighing ball-milled powder according to mass ratio, wherein three-dimensional graphene / MgAl2O4 10%-25%, Cu 0.5-1.5%, Mg 1%-2%, Si 0.3-1%, and the rest Al powder; mixing Cu, Mg, Si, Al and ethanol for high-energy ball milling, wherein the high-energy ball milling process is ball milling at a speed of 280-320 r / min for 8-10 h; then, adding three-dimensional graphene / MgAl2O4 and low-energy ball milling at a speed of 180-200 r / min for 3-9 h; after the ball milling is completed, vacuum drying; Step (5): cold isostatic pressing, the dried powder is loaded into a mold, sealed, and then put into a cold isostatic press for pressing and then demolding; Step (6): vacuum hot pressing, placing the cold isostatically pressed green body into a vacuum hot pressing furnace for hot pressing and sintering; The aluminum source and magnesium source are aluminum nitrate and magnesium nitrate respectively, and the ratio of aluminum nitrate, magnesium nitrate and diethanolamine is (0.02-0.04) mol: (0.01-0.02) mol: (8-30) mg; Vacuum hot pressing includes the following steps: 1) 20-40℃, evacuate for 1-3 hours, and the vacuum degree reaches 0.01-0.05Pa; 2) Heating to 300-500°C and pressurizing to 60-120MPa; 3) Raise the temperature to 400-600℃ and keep the temperature and pressure for 1-2 hours; 4) Cool to room temperature and take out the green body.

2. According to the method for preparing a high elastic modulus and high thermal conductivity aluminum-based composite material according to claim 1, the median particle size of the Al, Cu, Mg, and Si is 2 to 30 μm.

3. According to the method for preparing a high elastic modulus and high thermal conductivity aluminum-based composite material according to claim 1, the amount of ethanol added is 1-2 times the weight of the ball-milled powder.

4. According to the method for preparing a high elastic modulus and high thermal conductivity aluminum-based composite material according to claim 1, the mass ratio of ball milling powder to ball material is 1:10-1:20; and the ball milling protective atmosphere is argon.

5. According to the method for preparing an aluminum-based composite material with high elastic modulus and high thermal conductivity as claimed in claim 1, the vacuum degree of the vacuum drying in step (4) is 0.1-0.5 Pa and the drying temperature is 60-100°C.

6. According to the method for preparing a high elastic modulus and high thermal conductivity aluminum-based composite material according to claim 1, the cold isostatic pressing pressure in step (5) is 150-300 MPa, and the holding time is 10-30 min.

7. An aluminum-based composite material with high elastic modulus and high thermal conductivity, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Graphene modified high-heat-conductivity aluminum-based composite material and powder metallurgy preparation method

    CN104264000A

  • Light armored armor and preparation method thereof

    CN104848748A

  • Method for preparing graphene toughened silicon carbide ceramic composite material

    CN105801154A

  • A graphene-reinforced aluminum-based silicon carbide composite material, its preparation method, and its applications.

    CN106591666B

  • A graphene / silicon carbide reinforced aluminum matrix composite material and its preparation method

    CN108950280B