A production method of industrial pure iron wire rod for mine detonator blasting wire

Through the production method of industrial pure iron strips, using KR process and RH degassing processes, the problems of poor softness and unstable conductivity of low-carbon steel strips are solved, and the high rebound angle and conductivity are improved. Meet the technical indicators of mine detonator blasting lines and reduce production costs.

CN118460906BActive Publication Date: 2024-11-08JIANGSU YONGGANG GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410911967.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-08
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

The existing low-carbon steel strips have poor softness after processing, which is difficult to meet the high rebound angle and conductive performance requirements of the mine detonator blasting line. In addition, there are specification limitations and component fluctuations in the production process, resulting in unstable conductive performance.

Method used

Using the industrial pure iron strip production method, the chemical composition and rolling conditions are controlled through KR process desulfurization and iron smelting, RH degassing, continuous casting, grinding and high-pressure water phosphorus removal rolling, etc., to form fine grain size and high-pressure water The conductive strip meets the technical indicators of mine detonator blasting line.

Benefits of technology

The performance of the high rebound angle of the coil is stable ≥58°, the conductivity is in the range of 15.0-16.0%, and the tensile strength is 780-880MPa, which widens the raw material specifications, reduces production costs, and meets the technology of mine detonator blasting line Require.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118460906B_ABST
    Figure CN118460906B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of wire rod production, and specifically discloses a production method of an industrial pure iron wire rod for a mine detonator blasting line. The method comprises KR desulfurization, converter smelting, RH degassing, 160×160mm small square billet continuous casting, billet grinding, heating, rolling and Stellmo air cooling, thereby saving an LF furnace process and simultaneously changing a large square billet process to 160×160mm small square billet production, thereby saving a billet opening process and reducing production costs. The wire rod produced by the method meets the requirements of hot-rolled wire rod mechanical properties of 320±10Mpa, an area reduction rate of ≥50%, and a Brinell hardness of ≤260HBW, thereby being beneficial to the cold forming performance of the wire rod and broadening the raw material specifications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wire rod production, and in particular to a production method of industrial pure iron wire rod for mine detonator blasting wire. Background Art

[0002] Insulated wires for detonating electric detonators for engineering blasting that meet GB / T18014-2008 are generally made of copper core and galvanized steel core PVC insulated wires. However, in order to further reduce production costs and reduce the sensitivity of pure copper wires (civilian blasting), many manufacturers use low-carbon steel for alternative production. However, due to the special functionality and relatively complex use environment of blasting wires, the material is required to have good toughness and high and stable conductivity, as well as certain rebound strength requirements; after the finished product processing diameter reaches φ0.59mm wire diameter, it needs to have a stable rebound angle ≥58°, and the resistance must meet the requirements of 0.40-0.466Ω / m;

[0003] At present, most of the low-carbon steel wire rods used in blasting wires on the market have some problems that are difficult to overcome: 1. Generally, low-carbon steel wire rods have high deformation resistance and high hardening rate after drawing, resulting in poor softness of the finished wire, which is difficult to stably meet the standard requirement of springback angle <58°; 2. In order to avoid hardening rate, downstream processing technology often hopes that manufacturers can provide wire rods with specifications of ≤φ5.5mm, which has restrictions on specifications; 3. Generally, the composition of low-carbon steel products fluctuates greatly, making it difficult to guarantee the resistance requirements of users' conductive materials. Therefore, the market demand for materials with stable conductive properties and good drawing performance is particularly urgent. Summary of the invention

[0004] In view of the above problems, the present invention is proposed to provide a method for producing industrial pure iron wire rods for mine detonator blasting wires to overcome all or one of the above technical problems.

[0005] According to one aspect of the present invention, there is provided a method for producing industrial pure iron wire rod for mine detonator blasting wire, comprising the following steps:

[0006] Molten steel smelting: Desulfurized molten iron after the KR process is added into the converter for production to produce molten steel, and the chemical composition weight percentage of the molten steel is controlled within C≤0.04%, P≤0.015%; the dissolved oxygen of the steel is ≤800ppm;

[0007] RH degassing: The vacuum degree of RH furnace is controlled below 67Pa, maintained for more than 15 minutes, and the weight percentage of chemical composition of molten steel is controlled as follows: C: 0.002-0.010%, Si: ≤0.015%, Mn: 0.05-0.15%, P: ≤0.015%, S: ≤0.010%, N≤0.0030%, and the balance is iron and unavoidable impurities;

[0008] Before the molten steel is broken, Al particles are added for deoxidation to ensure that Al is ≤ 0.002% and dissolved oxygen is ≤ 20ppm; the soft blowing time at the bottom of the ladle is greater than 30 minutes;

[0009] Continuous casting produces billets: Continuous casting uses square billets with a cross-section of 160×160mm, uses integral nozzle casting, constant casting speed production, and controls the superheat to be stable at ≤40℃;

[0010] After the billet comes off the production line, it is ground to remove the defective layer on the billet surface;

[0011] Wire rod rolling: After the billet is heated to 1100-1150℃, high-pressure water is used to remove phosphorus and scale on the surface of the billet, and then the billet enters the rough rolling unit for rolling; after rough rolling, fine rolling is carried out, and the wire diameter of the wire rod is measured by an online diameter gauge;

[0012] Wire cooling: Close all insulation covers and cooling fans, and control the speed of the air cooling line roller to 0.30m / s.

[0013] Optionally, in the molten steel smelting process, low-carbon carbon scrap steel is selected and a top and bottom double blowing process is adopted; a slide plate is used to block slag when tapping the converter, and the tapping steel is directly covered with metallurgical lime and fluorite slag.

[0014] Optionally, the finishing rolling temperature is ≥960°C, and the finishing rolling adopts a finishing rolling unit and a sizing unit to roll and spin the wire, and the spinning temperature is controlled to be 910°C-950°C.

[0015] Optionally, the chemical composition and mass percentage of the industrial pure iron wire rod for mine detonator blasting line are: C: 0.0023%, Si: 0.007%, Mn: 0.07%, P: 0.008%, S: 0.006%, Al: 0.0015%, N: 0.0027%, and the remainder is iron and unavoidable impurities.

[0016] Optionally, the chemical composition and mass percentage of the industrial pure iron wire rod for mine detonator blasting line are: C: 0.0028%, Si: 0.006%, Mn: 0.08%, P: 0.007%, S: 0.006%, Al: 0.0018%, N: 0.0025%, and the remainder is iron and unavoidable impurities.

[0017] Optionally, the chemical composition and mass percentage of the industrial pure iron wire rod for mine detonator blasting line are: C: 0.0028%, Si: 0.005%, Mn: 0.075%, P: 0.005%, S: 0.005%, Al: 0.0014%, N: 0.0023%, and the remainder is iron and unavoidable impurities.

[0018] Optionally, the chemical composition and mass percentage of the industrial pure iron wire rod for mine detonator blasting line are: C: 0.010%, Si: 0.015%, Mn: 0.15%, P: 0.015%, S: 0.010%, Al: 0.002%, N: 0.003%, and the remainder is iron and unavoidable impurities.

[0019] Optionally, the chemical composition and mass percentage of the industrial pure iron wire rod for mine detonator blasting line are: C: 0.002%, Si: 0.010%, Mn: 0.05%, P: 0.010%, S: 0.007%, Al: 0.016%, N: 0.0030%, and the remainder is iron and unavoidable impurities.

[0020] The invention provides a production method of industrial pure iron wire rod for mine detonator blasting wire, which saves the LF furnace process and changes the large square billet process to 160×160mm small square billet production, thus saving the billet opening process, avoiding billet opening energy consumption and reducing production costs.

[0021] By adding Al for deoxidation before the molten steel breaks through the air, stable inclusions are formed with oxygen and nitrogen in the molten steel. Through the circulation of vacuum molten steel, large particle inclusions are floated and removed, and fine inclusions remain in the steel; the fine inclusions can pin the grain boundary, making the grain boundary more dense, and can also inhibit the trend of grain growth due to heat in the subsequent rolling process, so that a grain refinement structure can be obtained through rolling, and the grain size of the wire rod can reach level 5;

[0022] The wire rod produced by the production method proposed in this application meets the mechanical properties of hot-rolled wire rod of 320±10MPa, surface reduction rate ≥50%, Brinell hardness ≤260HBW, which is beneficial to the cold forming performance of wire rod and broadens the raw material specifications. Users can choose wire rod ≤φ6.5mm for production, which reduces production costs compared with the existing process; and the total oxygen content in the wire rod inspection steel is ≤50ppm, ensuring the material drawing effect; the electrical conductivity of the wire rod is stably controlled within the range of 15.0-16.0%, and after the wire rod is drawn and heat treated, the tensile strength of the finished blasting wire reaches 780-880MPa after the diameter reaches φ0.59mm, the rebound angle is stable ≥58°, and the resistance meets the requirements of 0.40-0.466Ω / m, which meets the technical index requirements of mine detonator blasting wire. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present invention. Moreover, the same reference symbols are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:

[0024] Figure 1 The metallographic structure diagram of the wire rod produced by the present invention is shown. DETAILED DESCRIPTION

[0025] The present invention is further described in detail below in conjunction with specific embodiments, but it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present invention and to fully convey the scope of the present invention to those skilled in the art. Example 1

[0026] The chemical composition and mass percentage of the industrial pure iron wire rod in this embodiment are: C: 0.0023%, Si: 0.007%, Mn: 0.07%, P: 0.008%, S: 0.006%, Al: 0.0015%, N: 0.0027%, and the remainder is iron and unavoidable impurities. The specification is φ6.5mm, and the specific production process is:

[0027] Molten steel smelting: Desulfurized molten iron after KR process is used and added to the converter for production. Self-produced low-carbon carbon scrap steel is selected, and the top and bottom double blowing process is adopted to maintain good bottom blowing conditions. The converter uses a slide plate to block the slag, and the steel is directly covered with metallurgical lime and fluorite slag to prevent slag. Steel tapping C: 0.035%, P: 0.007%; Dissolved oxygen in steel tapping is 760ppm;

[0028] RH degassing: The vacuum degree of the RH furnace is controlled at 66Pa for 20 minutes to control the composition of the molten steel to meet the standard;

[0029] Before the molten steel is broken, Al particles are added for deoxidation, Al: 0.0015%, dissolved oxygen 18ppm; the soft blowing time at the bottom of the ladle is 32 minutes to further reduce inclusions in the steel;

[0030] Continuous casting: Continuous casting is produced with square billets with a cross section of 160×160mm, using integral nozzle casting, constant casting speed, controlled superheat at 36°C, end electromagnetic stirring current of 550A and frequency of 10Hz, secondary cooling water volume of 1.4L / kg, and light pressure reduction of 8mm;

[0031] The billet is fully ground off the production line, using a 16-mesh grinding wheel for rough grinding and a 24-mesh grinding wheel for fine grinding, with a grinding depth of 1.5mm, to completely remove the defective layer on the billet surface, ensuring the billet surface quality;

[0032] The steel rolling adopts a walking beam heating furnace with a temperature difference of 27℃ in the cross section of the steel billet; the heating section is 1185℃, the soaking section is 1160℃, the starting rolling temperature is 1120℃, and the high-pressure water dephosphorization rolling is carried out with a dephosphorization pressure of 16MPa. After the iron oxide scale on the surface of the steel billet is removed, it enters the rough rolling unit for rolling to ensure the surface quality of the product; the finishing rolling adopts the Morgan finishing unit and the sizing unit for rolling control, and the online diameter gauge can realize timely and accurate measurement of the size to ensure that the wire rod size accuracy reaches C-level accuracy.

[0033] Controlled cooling: the finishing rolling temperature is 980℃; the wire laying temperature is controlled at 940℃, slow cooling is adopted after wire laying, the roller speed of the Stelmo air cooling line is set to 0.30m / s, the heat preservation cover is fully closed, the cooling fan is fully closed, and the coil is collected to avoid scratches. The mechanical properties and organization of the wire rod suitable for cold forming are obtained by optimizing the controlled cooling process.

[0034] The wire rod with a diameter of φ6.5 mm obtained by the above method has a microstructure as shown in the attached figure. Figure 1 As shown, it is mainly ferrite and the grain size is level 5.

[0035] The wire rod prepared by the above method, after drawing and heat treatment, has a finished blasting wire with a diameter of φ0.59mm, a tensile strength of 810MPa, a stable rebound angle of ≥59.5°, and a resistance of 0.455Ω / m. It complies with the national standard GB / T18014-2008 on polyvinyl chloride insulated wires for electric detonator detonation and meets the technical index requirements of mine detonator blasting wires. Example 2

[0036] The industrial pure iron wire rod in this embodiment has the following components: C: 0.0028%, Si: 0.006%, Mn: 0.08%, P: 0.007%, S: 0.006%, Al: 0.0018%, N: 0.0025%, and the remainder is iron and unavoidable impurities. The specification is φ6.5mm, and the specific production process is:

[0037] Molten steel smelting: Desulfurized molten iron after KR process is used and added to the converter for production. Self-produced low-carbon carbon scrap steel is selected, and the top and bottom double blowing process is adopted to maintain good bottom blowing conditions. The converter uses a slide plate to block the slag, and the tapping is directly covered with metallurgical lime and fluorite slag to prevent slag. Tapping C: 0.036%, P: 0.006%; tapping dissolved oxygen 760ppm;

[0038] RH degassing: The vacuum degree of the RH furnace is controlled at 65Pa for 19 minutes to control the composition of the molten steel to meet the standard;

[0039] Before the molten steel is broken, Al particles are added for deoxidation, Al: 0.0018%, dissolved oxygen 15ppm; the soft blowing time at the bottom of the ladle is 35 minutes to further reduce inclusions in the steel;

[0040] Continuous casting: Continuous casting is produced with square billets with a cross section of 160×160mm, using integral nozzle casting, constant casting speed, controlled superheat at 35°C, end electromagnetic stirring current of 550A, frequency of 10Hz, secondary cooling water volume of 1.4L / kg, and light pressure reduction of 8mm;

[0041] The billet is fully ground off the production line, using a 16-mesh grinding wheel for rough grinding and a 24-mesh grinding wheel for fine grinding, with a grinding depth of 1.5mm, to completely remove the defective layer on the billet surface, ensuring the billet surface quality;

[0042] The steel rolling adopts a walking beam heating furnace with a temperature difference of 25℃ in the cross section of the steel billet; the heating section is 1190℃, the soaking section is 1165℃, the starting rolling temperature is 1130℃, and the high-pressure water dephosphorization rolling is carried out with a dephosphorization pressure of 17MPa. After the iron oxide scale on the surface of the steel billet is removed, it enters the rough rolling unit for rolling to ensure the surface quality of the product; the finishing rolling adopts the Morgan finishing unit and the sizing unit for rolling control, and the online diameter gauge can be used to achieve timely and accurate measurement of the size to ensure that the wire rod size accuracy reaches C-level accuracy.

[0043] Controlled cooling: the finishing rolling temperature is 955℃; the wire laying temperature is controlled at 945℃, slow cooling is adopted after wire laying, the roller speed of the Stelmo air cooling line is set to 0.30m / s, the heat preservation cover is fully closed, the cooling fan is fully closed, and the coil is collected to avoid scratches. The mechanical properties and organization of the wire rod suitable for cold forming are obtained by optimizing the controlled cooling process.

[0044] The wire rod prepared by the above method, after drawing and heat treatment, has a finished blasting wire with a diameter of φ0.59mm, a tensile strength of 820MPa, a stable rebound angle of ≥61°, and a resistance of 0.446Ω / m. It complies with the national standard GB / T18014-2008 on polyvinyl chloride insulated wires for electric detonator detonation and meets the technical index requirements of mine detonator blasting wires. Example 3

[0045] The industrial pure iron wire rod in this embodiment has the following components: C: 0.0028%, Si: 0.005%, Mn: 0.075%, P: 0.005%, S: 0.005%, Al: 0.0014%, N: 0.0023%, and the remainder is iron and unavoidable impurities. The specification is φ6.5mm, and the specific production process is:

[0046] Molten steel smelting: Desulfurized molten iron after KR process is used and added to the converter for production. Self-produced low-carbon carbon scrap steel is selected, and the top and bottom double blowing process is adopted to maintain good bottom blowing conditions. The converter uses a slide plate to block the slag, and the tapping is directly covered with metallurgical lime and fluorite slag to prevent slag. Tapping C: 0.034%, P: 0.004%; tapping dissolved oxygen 743ppm;

[0047] RH degassing: The vacuum degree of the RH furnace is controlled at 62Pa for 21 minutes to control the composition of the molten steel to meet the standard;

[0048] Before the molten steel is broken, Al particles are added for deoxidation, Al: 0.0014%, dissolved oxygen 18ppm; the soft blowing time at the bottom of the ladle is 36 minutes to further reduce inclusions in the steel;

[0049] Continuous casting: Continuous casting is produced with square billets with a cross section of 160×160mm, using integral nozzle casting, constant casting speed, controlled superheat at 37°C, end electromagnetic stirring current of 550A, frequency of 10Hz, secondary cooling water volume of 1.4L / kg, and light pressure reduction of 8mm;

[0050] The billet is fully ground off the production line, using a 16-mesh grinding wheel for rough grinding and a 24-mesh grinding wheel for fine grinding, with a grinding depth of 1.5mm, to completely remove the defective layer on the billet surface, ensuring the billet surface quality;

[0051] The steel rolling adopts a walking beam heating furnace with a temperature difference of 27℃ in the cross section of the steel billet; the heating section is 1195℃, the soaking section is 1175℃, the starting rolling temperature is 1135℃, and the high-pressure water dephosphorization rolling is carried out with a dephosphorization pressure of 17MPa. After the iron oxide scale on the surface of the steel billet is removed, it enters the rough rolling unit for rolling to ensure the surface quality of the product; the finishing rolling adopts the Morgan finishing unit and the sizing unit for rolling control, and the online diameter gauge can realize timely and accurate measurement of the size to ensure that the wire rod size accuracy reaches C-level accuracy.

[0052] Controlled cooling: the finishing rolling temperature is 938℃; the wire laying temperature is controlled at 932℃, slow cooling is adopted after wire laying, the roller speed of the Stelmo air cooling line is set to 0.30m / s, the heat preservation cover is fully closed, the cooling fan is fully closed, and the coil is collected to avoid scratches. The mechanical properties and organization of the wire rod suitable for cold forming are obtained by optimizing the controlled cooling process.

[0053] The wire rod prepared by the above method, after drawing and heat treatment, has a finished blasting wire with a diameter of φ0.59mm, a tensile strength of 830MPa, a stable rebound angle of ≥61°, and a resistance of 0.443Ω / m. It complies with the national standard GB / T18014-2008 on polyvinyl chloride insulated wires for electric detonator detonation and meets the technical index requirements of mine detonator blasting wires. Example 4

[0054] The industrial pure iron wire rod in this embodiment has the following components: C: 0.010%, Si: 0.015%, Mn: 0.15%, P: 0.015%, S: 0.010%, Al: 0.002%, N: 0.003%, and the remainder is iron and unavoidable impurities. The specification is φ6.5mm, and the specific production process is:

[0055] Molten steel smelting: Desulfurized molten iron after KR process is used and added to the converter for production. Self-produced low-carbon carbon scrap steel is selected, and the top and bottom double blowing process is adopted to maintain good bottom blowing conditions. The converter uses a slide plate to block the slag, and the tapping is directly covered with metallurgical lime and fluorite slag to prevent slag. Tapping C: 0.034%, P: 0.004%; tapping dissolved oxygen 743ppm;

[0056] RH degassing: The vacuum degree of the RH furnace is controlled at 62Pa for 21 minutes to control the composition of the molten steel to meet the standard;

[0057] Before the molten steel is broken, Al particles are added for deoxidation, Al: 0.002%, dissolved oxygen 16ppm; the soft blowing time at the bottom of the ladle is 40 minutes to further reduce inclusions in the steel;

[0058] Continuous casting: Continuous casting is produced with square billets with a cross section of 160×160mm, using integral nozzle casting, constant casting speed, controlled superheat at 37°C, end electromagnetic stirring current of 550A, frequency of 10Hz, secondary cooling water volume of 1.4L / kg, and light pressure reduction of 8mm;

[0059] The billet is fully ground off the production line, using a 16-mesh grinding wheel for rough grinding and a 24-mesh grinding wheel for fine grinding, with a grinding depth of 1.5mm, to completely remove the defective layer on the billet surface, ensuring the billet surface quality;

[0060] The steel rolling adopts a walking beam heating furnace with a temperature difference of 27℃ in the cross section of the steel billet; the heating section is 1195℃, the soaking section is 1175℃, the starting rolling temperature is 1135℃, and the high-pressure water dephosphorization rolling is carried out with a dephosphorization pressure of 17MPa. After the iron oxide scale on the surface of the steel billet is removed, it enters the rough rolling unit for rolling to ensure the surface quality of the product; the finishing rolling adopts the Morgan finishing unit and the sizing unit for rolling control, and the online diameter gauge can realize timely and accurate measurement of the size to ensure that the wire rod size accuracy reaches C-level accuracy.

[0061] Controlled cooling: the finishing rolling temperature is 938℃; the wire laying temperature is controlled at 932℃, slow cooling is adopted after wire laying, the roller speed of the Stelmo air cooling line is set to 0.30m / s, the heat preservation cover is fully closed, the cooling fan is fully closed, and the coil is collected to avoid scratches. The mechanical properties and organization of the wire rod suitable for cold forming are obtained by optimizing the controlled cooling process.

[0062] The wire rod prepared by the above method, after drawing and heat treatment, has a finished blasting wire with a diameter of φ0.59mm, a tensile strength of 840MPa, a stable rebound angle of ≥60°, and a resistance of 0.436Ω / m. It complies with the national standard GB / T18014-2008 on polyvinyl chloride insulated wires for electric detonator detonation and meets the technical index requirements of mine detonator blasting wires. Example 5

[0063] The industrial pure iron wire rod in this embodiment has the following components: C: 0.002%, Si: 0.010%, Mn: 0.05%, P: 0.010%, S: 0.007%, Al: 0.016%, N: 0.0030%, and the remainder is iron and unavoidable impurities. The specification is φ6.5mm, and the specific production process is:

[0064] Molten steel smelting: Desulfurized molten iron after KR process is used and added to the converter for production. Self-produced low-carbon carbon scrap steel is selected, and the top and bottom double blowing process is adopted to maintain good bottom blowing conditions. The converter uses a slide plate to block the slag, and the tapping is directly covered with metallurgical lime and fluorite slag to prevent slag. Tapping C: 0.034%, P: 0.004%; tapping dissolved oxygen 743ppm;

[0065] RH degassing: The vacuum degree of the RH furnace is controlled at 64Pa for 21 minutes to control the composition of the molten steel to meet the standard;

[0066] Before the molten steel is broken, Al particles are added for deoxidation, Al: 0.016%, dissolved oxygen 18ppm; the ladle bottom soft blowing time is 35 minutes to further reduce inclusions in the steel;

[0067] Continuous casting: Continuous casting is produced with square billets with a cross section of 160×160mm, using integral nozzle casting, constant casting speed, controlled superheat at 37°C, end electromagnetic stirring current of 550A, frequency of 10Hz, secondary cooling water volume of 1.4L / kg, and light pressure reduction of 8mm;

[0068] The billet is fully ground off the production line, using a 16-mesh grinding wheel for rough grinding and a 24-mesh grinding wheel for fine grinding, with a grinding depth of 1.5mm, to completely remove the defective layer on the billet surface, ensuring the billet surface quality;

[0069] The steel rolling adopts a walking beam heating furnace with a temperature difference of 27℃ in the cross section of the steel billet; the heating section is 1195℃, the soaking section is 1175℃, the starting rolling temperature is 1135℃, and the high-pressure water dephosphorization rolling is carried out with a dephosphorization pressure of 17MPa. After the iron oxide scale on the surface of the steel billet is removed, it enters the rough rolling unit for rolling to ensure the surface quality of the product; the finishing rolling adopts the Morgan finishing unit and the sizing unit for rolling control, and the online diameter gauge can realize timely and accurate measurement of the size to ensure that the wire rod size accuracy reaches C-level accuracy.

[0070] Controlled cooling: the finishing rolling temperature is 938℃; the wire laying temperature is controlled at 932℃, slow cooling is adopted after wire laying, the roller speed of the Stelmo air cooling line is set to 0.30m / s, the heat preservation cover is fully closed, the cooling fan is fully closed, and the coil is collected to avoid scratches. The mechanical properties and organization of the wire rod suitable for cold forming are obtained by optimizing the controlled cooling process.

[0071] The wire rod prepared by the above method, after drawing and heat treatment, has a finished blasting wire with a diameter of φ0.59mm, a tensile strength of 850MPa, a stable rebound angle of ≥59°, and a resistance of 0.438Ω / m. It complies with the national standard GB / T18014-2008 on polyvinyl chloride insulated wires for electric detonator detonation and meets the technical index requirements of mine detonator blasting wires.

[0072] The existing technology for producing wire rod generally adopts molten iron pretreatment → converter smelting → LF refining → RH degassing → billet continuous casting → billet opening → grinding → billet heating in heating furnace → high-speed wire rolling → laying head → Stelmo air cooling → packaging → finished product;

[0073] The present application adopts molten iron pretreatment → converter smelting → RH degassing → billet continuous casting → grinding → heating furnace billet heating → high-speed wire rolling → laying head → Stelmo air cooling → packaging → finished product.

[0074] The LF furnace process is saved, and the large billet process is changed to 160×160mm small billet production, which also saves the billet opening process, avoids billet opening energy consumption, and reduces production costs;

[0075] The performance test results of the wire rods produced in Examples 1-5 are shown in Table 1;

[0076] Table 1

[0077]

[0078] Among them, the tensile strength and cross-sectional shrinkage rate are measured using the markings and methods of GB / T228.1-2010 "Tensile Test of Metal Materials", the total oxygen content is measured using the method in GB / T11261-2006 "Determination of Oxygen Content of Steel", the Brinell hardness is measured using the method and standards of GB / T231.1-2018 "Brinell Hardness Test of Metal Materials", and the conductivity is measured using the method of GB / T351-2019 "Method for Measuring Resistivity of Metal Materials".

[0079] It can be seen from Table 1 that the wire rod produced by the production method proposed in this application meets the mechanical properties of hot-rolled wire rod of 320±10MPa, surface reduction rate ≥50%, Brinell hardness ≤260HBW, which is beneficial to the cold forming performance of wire rod and broadens the raw material specifications. Users can choose wire rod ≤φ6.5mm for production, which reduces production costs compared with the existing process; and the total oxygen content in the wire rod inspection steel is ≤50ppm, which ensures the material drawing effect; the electrical conductivity of the wire rod is stably controlled within the range of 15.0-16.0%, and after the wire rod is drawn and heat treated, the tensile strength of the finished blasting wire reaches 780-880MPa after the diameter reaches φ0.59mm, the rebound angle is stable ≥58°, and the resistance meets the requirements of 0.40-0.466Ω / m, which meets the technical index requirements of mine detonator blasting wire.

[0080] In the description provided herein, a large number of specific details are described. However, it is understood that embodiments of the present invention can be practiced without these specific details. In some instances, well-known methods, structures and techniques are not shown in detail so as not to obscure the understanding of this description.

Claims

1. A method for producing industrial pure iron wire rod for mine detonator blasting wire, characterized in that: The steps include: Molten steel smelting: Desulfurized molten iron that has gone through the KR process is added to the converter for production to produce molten steel, and the chemical composition weight percentage of the molten steel is controlled at C≤0.04%, P≤0.015%; the dissolved oxygen in the steel is ≤800ppm, low-carbon carbon scrap steel is selected, and the top and bottom double blowing process is adopted; the converter uses a slide plate to block the slag, and the steel is directly covered with metallurgical lime and fluorite slag; RH degassing: The vacuum degree of RH furnace is controlled below 67Pa, maintained for more than 15 minutes, and the weight percentage of chemical composition of molten steel is controlled as follows: C: 0.002-0.010%, Si: ≤0.015%, Mn: 0.05-0.15%, P: ≤0.015%, S: ≤0.010%, N≤0.0030%, and the balance is iron and unavoidable impurities; Before the molten steel is broken, Al particles are added for deoxidation to ensure that Al is ≤ 0.002% and dissolved oxygen is ≤ 20ppm; the soft blowing time at the bottom of the ladle is greater than 30 minutes; Continuous casting produces billets: Continuous casting uses square billets with a cross-section of 160×160mm, uses integral nozzle casting, constant casting speed production, and controls the superheat to be stable at ≤40℃; After the billet comes off the production line, it is ground to remove the defective layer on the billet surface; Wire rolling: After the billet is heated to 1100-1150℃, high-pressure water is used to remove phosphorus and scale on the surface of the billet, and then the billet enters the rough rolling unit for rolling; after rough rolling, finishing rolling is carried out, and the wire diameter of the wire rod is measured by an online diameter gauge. The finishing rolling temperature is ≥960℃. The finishing rolling uses a finishing rolling unit and a sizing unit for rolling and spinning, and the spinning temperature is controlled at 910℃-950℃; Wire cooling: The wire is naturally cooled in the protective cover to obtain a finished wire rod. After the finished wire rod is drawn and heat treated, the diameter of the finished blasting wire reaches φ0.59mm, and the rebound angle is stable ≥58°.

2. The method for producing industrial pure iron wire rod for mine detonator blasting wire according to claim 1, characterized in that: The chemical composition and mass percentage of the industrial pure iron wire rod for mine detonator blasting wire are: C: 0.0023%, Si: 0.007%, Mn: 0.07%, P: 0.008%, S: 0.006%, Al: 0.0015%, N: 0.0027%, and the remainder is iron and unavoidable impurities.

3. The method for producing industrial pure iron wire rod for mine detonator blasting wire according to claim 1, characterized in that: The chemical composition and mass percentage of the industrial pure iron wire rod for mine detonator blasting wire are: C: 0.0028%, Si: 0.006%, Mn: 0.08%, P: 0.007%, S: 0.006%, Al: 0.0018%, N: 0.0025%, and the remainder is iron and unavoidable impurities.

4. The method for producing industrial pure iron wire rod for mine detonator blasting wire according to claim 1, characterized in that: The chemical composition and mass percentage of the industrial pure iron wire rod for mine detonator blasting wire are: C: 0.0028%, Si: 0.005%, Mn: 0.075%, P: 0.005%, S: 0.005%, Al: 0.0014%, N: 0.0023%, and the balance is iron and unavoidable impurities.

5. The method for producing industrial pure iron wire rod for mine detonator blasting wire according to claim 1, characterized in that: The chemical composition and mass percentage of the industrial pure iron wire rod for mine detonator blasting wire are: C: 0.010%, Si: 0.015%, Mn: 0.15%, P: 0.015%, S: 0.010%, Al: 0.002%, N: 0.003%, and the balance is iron and unavoidable impurities.

6. The method for producing industrial pure iron wire rod for mine detonator blasting wire according to claim 1, characterized in that: The chemical composition and mass percentage of the industrial pure iron wire rod for mine detonator blasting wire are: C: 0.002%, Si: 0.010%, Mn: 0.05%, P: 0.010%, S: 0.007%, Al: 0.016%, N: 0.0030%, and the remainder is iron and unavoidable impurities.