Antistatic polystyrene material and preparation method thereof

By adding polymethacrylic nanomicrospheres loaded with nanographite phase carbon nitride to polystyrene and using electrospinning technology, the problems of poor binding force and failure in use of antistatic materials are solved, and better resistance is achieved Electrostatic and mechanical properties.

CN118461162BActive Publication Date: 2024-11-22WUJIANG BODA ELECTRONICS TECH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410521434.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-28
Publication Date
2024-11-22
Estimated Expiration
2044-04-28

AI Technical Summary

Technical Problem

Existing antistatic materials are prone to failure during use, and the nanographite phase carbon nitride bonds with polystyrene, resulting in poor antistatic effect.

Method used

Add polymethacrylic nanomicrospheres loaded with nanographite phase carbon nitride to polystyrene, and anti-static polystyrene materials are prepared through electrospinning technology, using amino groups and ordered tris-s of nanographite phase carbon nitride to use nanographite phase carbon nitride to prepare - Triazine unit receives protons to achieve electrostatic dissipation, improves the antistatic properties of the material, and enhances the dispersion and binding force of the nanographite phase carbon nitride through polymethacrylic nanomicrospheres.

Benefits of technology

It effectively improves the antistatic effect of polystyrene, enhances the mechanical properties of the material, including tensile strength and notch impact strength, and solves the problems of carbon nitride agglomeration and poor binding force of nanographite phase.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004815228160000041
    Figure BDA0004815228160000041
  • Figure BDA0004815228160000061
    Figure BDA0004815228160000061
  • Figure BDA0004815228160000071
    Figure BDA0004815228160000071
Patent Text Reader

Abstract

The present invention provides an antistatic polystyrene material and a preparation method thereof. The steps are as follows: S1: dispersing polymethacrylic acid nano-microspheres loaded with nano-graphite phase carbon nitride in acetone, and mixing by magnetic stirring; S2: adding polystyrene, continuing magnetic stirring for 15 hours, and obtaining a uniform mixed solution; S3: transferring the mixed solution to an electrostatic spinning device, and performing electrostatic spinning to obtain an antistatic polystyrene material. The present invention adds nano-graphite phase carbon nitride to polystyrene, and since the amino groups on the surface of the graphite phase carbon nitride and the ordered tri-s-triazine units carry six nitrogen lone pairs of electrons, they have the ability to receive protons, and can achieve an electrostatic dissipation effect through the transfer of internal protons, which can effectively improve the antistatic effect of polystyrene.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of blister materials, and in particular to an antistatic polystyrene material and a preparation method thereof. Background Art

[0002] When antistatic agents are used conventionally, they need to have appropriate compatibility with plastics to ensure that an appropriate amount of antistatic agents migrate from the inside of the plastic to the surface to achieve a certain surface concentration, showing excellent antistatic effects. In addition, after the antistatic agents on the surface are removed by solvent washing or friction during use, they can quickly migrate from the inside to the surface to restore their antistatic effects. However, this method requires qualitative judgment based on the appropriate difference in polarity or solubility parameters between the antistatic agent and the plastic molecules, which is very cumbersome and sometimes fails to achieve the expected effect. At the same time, with the disappearance of the antistatic component, the antistatic effect of the material cannot be guaranteed.

[0003] Nano-graphite carbon nitride has good conductivity and can greatly improve its antistatic properties when combined with a polystyrene substrate. However, due to its small particle size, it is easy to agglomerate and has poor bonding with the polystyrene substrate. Therefore, it must be treated accordingly to improve its dispersibility and bonding ability with the polystyrene substrate. Summary of the invention

[0004] Technical problem to be solved: The purpose of the present invention is to provide an antistatic polystyrene material and a preparation method thereof, wherein nanographite phase carbon nitride is added to polystyrene. Since the amino groups on the surface of the graphite phase carbon nitride and the ordered tri-s-triazine units carry six nitrogen lone pairs of electrons and have the ability to receive protons, the electrostatic dissipation effect can be achieved through the transfer of internal protons, thereby effectively improving the antistatic effect of polystyrene.

[0005] Technical solution: A method for preparing an antistatic polystyrene material, the preparation steps are as follows:

[0006] S1: Disperse polymethacrylic acid nanospheres loaded with nanographite carbon nitride in acetone and mix them by magnetic stirring;

[0007] S2: Add polystyrene and continue magnetic stirring for 15 h to obtain a uniform mixed solution;

[0008] S3: transferring the mixed solution to an electrospinning device for electrospinning to obtain an antistatic polystyrene material.

[0009] Furthermore, the particle size of the polymethacrylic acid nano-microspheres loaded with nano-graphite phase carbon nitride is 800-980nm.

[0010] Furthermore, the preparation method of the polymethacrylic acid nano-microspheres loaded with nano-graphite phase carbon nitride is as follows:

[0011] S11: Take 2-5 parts of nano-graphite phase carbon nitride, add 100-120 parts of toluene, heat to boiling, introduce N2, add 5-6 parts of hydrolyzed silane coupling agent, and stir to react for 4-5 hours;

[0012] S12: repeatedly washing with ethanol, filtering, and drying to obtain modified nano-graphite phase carbon nitride;

[0013] S13: Take the modified nano-graphite phase carbon nitride, add 100-120 parts of toluene solution, introduce N2, stir at 100 rpm for 5-10 min, heat to 80°C, add 0.3-0.6 parts of initiator BPO, then add 80-90 parts of methacrylic acid, and react at high speed stirring for 3 hours;

[0014] S14: Filter and wash with acetone to obtain.

[0015] Furthermore, the particle size of the nano-graphite phase carbon nitride is 30-80 nm.

[0016] Furthermore, the rotation speed of the high-speed stirring is 350-450 rpm.

[0017] Furthermore, the mass volume ratio of the polymethacrylic acid nano-microspheres loaded with nano-graphite phase carbon nitride, polystyrene and acetone is (2-3) g: (13-15) g: 80 mL.

[0018] Further, the electrospinning parameters are: the spinning temperature is 22-28°C, the spinning voltage is 14-15kV, the relative humidity is 40-50%, the receiving distance between the receiving plate and the electrospinning nozzle device is 10-12cm, and the spinning solution flow rate is 1.0-1.5mL / h. Further, the inner diameter of the electrospinning nozzle in S6 is 0.5-0.86mm.

[0019] The antistatic polystyrene material prepared by the above preparation method.

[0020] Beneficial effects:

[0021] 1. The present invention adds nano-graphite phase carbon nitride to polystyrene. Since the amino groups on the surface of the graphite phase carbon nitride and the ordered tri-s-triazine units carry six nitrogen lone pairs of electrons and have the ability to receive protons, the electrostatic dissipation effect can be achieved through the transfer of internal protons, which can effectively improve the antistatic effect of polystyrene.

[0022] 2. Since the nano-graphite carbon nitride has a small particle size, it is easy to agglomerate and has a very poor bonding force with the polystyrene substrate. The present invention loads it on polymethacrylic acid nano-microspheres, which can effectively solve the problems of nano-graphite carbon nitride agglomeration and poor bonding with the polystyrene substrate, which affect the mechanical properties of polystyrene. At the same time, the polymethacrylic acid nano-microspheres have good hydrophilicity and can absorb or associate water molecules in the air through the hydrophilic groups on the main chain of the macromolecule, forming a conductive water film on the surface of the polystyrene to dissipate static charge, further improving the antistatic effect of the material.

[0023] 3. The polymethacrylic acid nano-microspheres loaded with nano-graphite phase carbon nitride of the present invention are well combined with polystyrene, and even within a certain amount of addition range, some mechanical properties, including tensile strength and notched impact strength, can be improved. DETAILED DESCRIPTION

[0024] The present invention proposes an antistatic polystyrene material and a preparation method thereof. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention will be further described in detail with reference to the following embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0025] Example 1

[0026] The preparation method of polymethacrylic acid nano-microspheres loaded with nano-graphite phase carbon nitride is as follows:

[0027] S11: Take 2 parts of nano-graphite phase carbon nitride with a particle size of 30-80 nm, add 100 parts of toluene, heat to boiling, introduce N2, add 5 parts of hydrolyzed silane coupling agent KH550, and stir to react for 4 hours;

[0028] S12: repeatedly washing with ethanol, filtering, and drying to obtain modified nano-graphite phase carbon nitride;

[0029] S13: Take the modified nano-graphite phase carbon nitride, add 100 parts of toluene solution, introduce N2, stir at 100 rpm for 5 min, heat to 80°C, add 0.3 parts of initiator BPO, then add 80 parts of methacrylic acid, and stir at 350 rpm for 3 h;

[0030] S14: Filter and wash with acetone to obtain.

[0031] Example 2

[0032] The preparation method of polymethacrylic acid nano-microspheres loaded with nano-graphite phase carbon nitride is as follows:

[0033] S11: Take 3 parts of nano-graphite phase carbon nitride with a particle size of 30-80 nm, add 110 parts of toluene, heat to boiling, introduce N2, add 5 parts of hydrolyzed silane coupling agent KH550, and stir to react for 4.5 hours;

[0034] S12: repeatedly washing with ethanol, filtering, and drying to obtain modified nano-graphite phase carbon nitride;

[0035] S13: Take the modified nano-graphite phase carbon nitride, add 110 parts of toluene solution, introduce N2, stir at 100 rpm for 6 min, heat to 80°C, add 0.4 parts of initiator BPO, then add 85 parts of methacrylic acid, and stir at 400 rpm for 3 h;

[0036] S14: Filter and wash with acetone to obtain.

[0037] Example 3

[0038] The preparation method of polymethacrylic acid nano-microspheres loaded with nano-graphite phase carbon nitride is as follows:

[0039] S11: Take 4 parts of nanographite carbon nitride with a particle size of 30-80 nm, add 110 parts of toluene, heat to boiling, introduce N2, add 6 parts of hydrolyzed silane coupling agent KH550, and stir to react for 4.5 hours;

[0040] S12: repeatedly washing with ethanol, filtering, and drying to obtain modified nano-graphite phase carbon nitride;

[0041] S13: Take the modified nano-graphite phase carbon nitride, add 110 parts of toluene solution, introduce N2, stir at 100 rpm for 7 min, heat to 80°C, add 0.5 parts of initiator BPO, then add 85 parts of methacrylic acid, and stir at 400 rpm for 3 h;

[0042] S14: Filter and wash with acetone to obtain.

[0043] Example 4

[0044] The preparation method of polymethacrylic acid nano-microspheres loaded with nano-graphite phase carbon nitride is as follows:

[0045] S11: Take 4 parts of nanographite carbon nitride with a particle size of 30-80 nm, add 110 parts of toluene, heat to boiling, introduce N2, add 6 parts of hydrolyzed silane coupling agent KH550, and stir to react for 4.5 hours;

[0046] S12: repeatedly washing with ethanol, filtering, and drying to obtain modified nano-graphite phase carbon nitride;

[0047] S13: Take the modified nano-graphite phase carbon nitride, add 110 parts of toluene solution, introduce N2, stir at 100 rpm for 9 minutes, heat to 80°C, add 0.5 parts of initiator BPO, and then add 85 parts of methacrylic acid, stir and react at 400 rpm for 3 hours;

[0048] S14: Filter and wash with acetone to obtain.

[0049] Example 5

[0050] The preparation method of polymethacrylic acid nano-microspheres loaded with nano-graphite phase carbon nitride is as follows:

[0051] S11: Take 5 parts of nano-graphite phase carbon nitride with a particle size of 30-80 nm, add 120 parts of toluene, heat to boiling, introduce N2, add 6 parts of hydrolyzed silane coupling agent KH550, and stir to react for 5 hours;

[0052] S12: repeatedly washing with ethanol, filtering, and drying to obtain modified nano-graphite phase carbon nitride;

[0053] S13: Take the modified nano-graphite phase carbon nitride, add 120 parts of toluene solution, introduce N2, stir at 100 rpm for 10 min, heat to 80°C, add 0.6 parts of initiator BPO, then add 90 parts of methacrylic acid, and stir at 450 rpm for 3 h;

[0054] S14: Filter and wash with acetone to obtain.

[0055] The particle size of the polymethacrylic acid nano-microspheres loaded with nano-graphite phase carbon nitride and the loading rate of nano-graphite phase carbon nitride in the above embodiment were measured, and the results are shown in Table 1 below:

[0056] Table 1

[0057]

[0058] Taking into account the particle size and nano-graphite phase carbon nitride loading rate, Example 4 was selected for subsequent experiments.

[0059] Example 6

[0060] A method for preparing an antistatic polystyrene material, the preparation steps are as follows:

[0061] S1: Take 2 g of the polymethacrylic acid nanospheres loaded with nano-graphite phase carbon nitride prepared in Example 4 and disperse them in 80 mL of acetone, and mix them by magnetic stirring;

[0062] S2: Add 13 g of polystyrene and continue magnetic stirring for 15 h to obtain a uniform mixed solution;

[0063] S3: The mixed solution is transferred to an electrospinning device for electrospinning. The electrospinning parameters are as follows: the spinning temperature is 22°C, the spinning voltage is 14 kV, the relative humidity is 40%, the receiving distance between the receiving plate and the electrospinning nozzle device is 10 cm, the inner diameter of the electrospinning nozzle is 0.5 mm, and the spinning solution flow rate is 1.0 mL / h, thereby obtaining an antistatic polystyrene material.

[0064] Example 7

[0065] A method for preparing an antistatic polystyrene material, the preparation steps are as follows:

[0066] S1: Take 2.5 g of the polymethacrylic acid nanospheres loaded with nano-graphite phase carbon nitride prepared in Example 4 and disperse them in 80 mL of acetone, and mix them by magnetic stirring;

[0067] S2: Add 13.5 g of polystyrene and continue magnetic stirring for 15 h to obtain a uniform mixed solution;

[0068] S3: The mixed solution is transferred to an electrospinning device for electrospinning. The electrospinning parameters are as follows: the spinning temperature is 28°C, the spinning voltage is 14 kV, the relative humidity is 45%, the receiving distance between the receiving plate and the electrospinning nozzle device is 11 cm, the inner diameter of the electrospinning nozzle is 0.6 mm, and the spinning solution flow rate is 1.2 mL / h, thereby obtaining an antistatic polystyrene material.

[0069] Example 8

[0070] A method for preparing an antistatic polystyrene material, the preparation steps are as follows:

[0071] S1: Take 2.5 g of the polymethacrylic acid nanospheres loaded with nano-graphite phase carbon nitride prepared in Example 4 and disperse them in 80 mL of acetone, and mix them by magnetic stirring;

[0072] S2: Add 14 g of polystyrene and continue magnetic stirring for 15 h to obtain a uniform mixed solution;

[0073] S3: The mixed solution is transferred to an electrospinning device for electrospinning. The electrospinning parameters are as follows: the spinning temperature is 28°C, the spinning voltage is 15 kV, the relative humidity is 45%, the receiving distance between the receiving plate and the electrospinning nozzle device is 11 cm, the inner diameter of the electrospinning nozzle is 0.67 mm, and the spinning solution flow rate is 1.3 mL / h, thereby obtaining an antistatic polystyrene material.

[0074] Example 9

[0075] A method for preparing an antistatic polystyrene material, the preparation steps are as follows:

[0076] S1: Take 2.5 g of the polymethacrylic acid nanospheres loaded with nano-graphite phase carbon nitride prepared in Example 4 and disperse them in 80 mL of acetone, and mix them by magnetic stirring;

[0077] S2: Add 14.5 g of polystyrene and continue magnetic stirring for 15 h to obtain a uniform mixed solution;

[0078] S3: The mixed solution is transferred to an electrospinning device for electrospinning. The electrospinning parameters are as follows: the spinning temperature is 28°C, the spinning voltage is 15 kV, the relative humidity is 45%, the receiving distance between the receiving plate and the electrospinning nozzle device is 11 cm, the inner diameter of the electrospinning nozzle is 0.67 mm, and the spinning solution flow rate is 1.4 mL / h, thereby obtaining an antistatic polystyrene material.

[0079] Example 10

[0080] A method for preparing an antistatic polystyrene material, the preparation steps are as follows:

[0081] S1: 3 g of polymethacrylic acid nanospheres loaded with nano-graphite phase carbon nitride prepared in Example 4 were dispersed in 80 mL of acetone and mixed by magnetic stirring;

[0082] S2: Add 15 g of polystyrene and continue magnetic stirring for 15 h to obtain a uniform mixed solution;

[0083] S3: The mixed solution is transferred to an electrospinning device for electrospinning. The electrospinning parameters are as follows: the spinning temperature is 28°C, the spinning voltage is 15 kV, the relative humidity is 50%, the receiving distance between the receiving plate and the electrospinning nozzle device is 12 cm, the inner diameter of the electrospinning nozzle is 0.86 mm, and the spinning solution flow rate is 1.5 mL / h, thereby obtaining an antistatic polystyrene material.

[0084] Comparative Example 1

[0085] The difference between this embodiment and embodiment 8 is that nano-graphite phase carbon nitride is directly added, and the polymethacrylic acid nano-microspheres loaded with an equal amount of nano-graphite phase carbon nitride are replaced by nano-graphite phase carbon nitride, specifically:

[0086] A method for preparing an antistatic polystyrene material, the preparation steps are as follows:

[0087] S1: Disperse 2.5 g of nano-graphite carbon nitride in 80 mL of acetone and mix by magnetic stirring;

[0088] S2: Add 14 g of polystyrene and continue magnetic stirring for 15 h to obtain a uniform mixed solution;

[0089] S3: The mixed solution is transferred to an electrospinning device for electrospinning. The electrospinning parameters are as follows: the spinning temperature is 28°C, the spinning voltage is 15 kV, the relative humidity is 45%, the receiving distance between the receiving plate and the electrospinning nozzle device is 11 cm, the inner diameter of the electrospinning nozzle is 0.67 mm, and the spinning solution flow rate is 1.3 mL / h, thereby obtaining an antistatic polystyrene material.

[0090] Comparative Example 2

[0091] The difference between this embodiment and embodiment 8 is that the polymethacrylic acid nano-microspheres loaded with nano-graphene are used instead of the polymethacrylic acid nano-microspheres loaded with nano-graphite carbon nitride, specifically:

[0092] A method for preparing an antistatic polystyrene material, the preparation steps are as follows:

[0093] S1: Disperse 2.5 g of polymethacrylic acid nanospheres loaded with nanographene in 80 mL of acetone and stir magnetically to mix; S2: Add 14 g of polystyrene and continue stirring magnetically for 15 h to obtain a uniform mixed solution;

[0094] S3: The mixed solution is transferred to an electrospinning device for electrospinning. The electrospinning parameters are as follows: the spinning temperature is 28°C, the spinning voltage is 15 kV, the relative humidity is 45%, the receiving distance between the receiving plate and the electrospinning nozzle device is 11 cm, the inner diameter of the electrospinning nozzle is 0.67 mm, and the spinning solution flow rate is 1.3 mL / h, thereby obtaining an antistatic polystyrene material.

[0095] The preparation method of polymethacrylic acid nano-microspheres loaded with nano-graphene is as follows:

[0096] S11: Take 4 parts of nanographene with a particle size of 30-80 nm, add 110 parts of toluene, heat to boiling, introduce N2, add 6 parts of hydrolyzed silane coupling agent KH550, and stir to react for 4.5 hours;

[0097] S12: repeatedly washing with ethanol, filtering, and drying to obtain modified nano-graphite phase carbon nitride;

[0098] S13: Take the modified nano-graphite phase carbon nitride, add 110 parts of toluene solution, introduce N2, stir at 100 rpm for 9 minutes, heat to 80°C, add 0.5 parts of initiator BPO, and then add 85 parts of methacrylic acid, stir and react at 400 rpm for 3 hours;

[0099] S14: Filter and wash with acetone to obtain.

[0100] Performance Testing:

[0101] The antistatic polystyrene materials prepared in each embodiment need to be treated with constant temperature and humidity before testing. The parameters of the constant temperature and humidity box are RH 50%, 25° C., and the required samples are made.

[0102] Surface resistance / volume resistivity test: The sample size is 10mm×10mm×2mm, and the sample is treated at a constant temperature and humidity for 48 hours.

[0103] Table 2

[0104]

[0105]

[0106] Tensile properties test: tested according to GB / T 1040-2018, the tensile rate is 50mm / min, the sample size is 170mm×10mm×4mm, and the sample is treated at constant temperature and humidity for 24h.

[0107] Notched impact performance test: Tested according to GB / T 1843-2008, the sample size is 80mm×10mm×4mm, the notch is type A, and the sample is treated at constant temperature and humidity for 24 hours.

[0108] Table 3

[0109]

Claims

1. A method for preparing an antistatic polystyrene material, It is characterized in that The preparation steps are as follows: S1: Disperse polymethacrylic acid nano-microspheres loaded with nano-graphite carbon nitride in acetone and mix them evenly by magnetic stirring; the mass volume ratio of the polymethacrylic acid nano-microspheres loaded with nano-graphite carbon nitride, polystyrene and acetone is (2-3) g: (13-15) g: 80 mL; S2: Add polystyrene and continue magnetic stirring for 15 h to obtain a uniform mixed solution; S3: transferring the mixed solution to an electrospinning device for electrospinning to obtain an antistatic polystyrene material; The preparation method of the polymethacrylic acid nano-microspheres loaded with nano-graphite phase carbon nitride is as follows: S11: Take 2-5 parts of nano-graphite carbon nitride, add 100-120 parts of toluene, heat to boiling, and pass N 2 , add 5-6 parts of hydrolyzed silane coupling agent and stir to react for 4-5 hours; S12: repeatedly washing with ethanol, filtering, and drying to obtain modified nano-graphite phase carbon nitride; S13: Take the modified nano-graphite phase carbon nitride, add 100-120 parts of toluene solution, and pass N 2 , stir at 100 rpm for 5-10 min, heat to 80°C, add 0.3-0.6 parts of initiator BPO, then add 80-90 parts of methacrylic acid, and react at high speed stirring for 3 hours; S14: Filter and wash with acetone to obtain.

2. The method for preparing an antistatic polystyrene material according to claim 1, Features: The particle size of the polymethacrylic acid nano-microspheres loaded with nano-graphite phase carbon nitride is 800-980nm.

3. The method for preparing an antistatic polystyrene material according to claim 1, Features: The particle size of the nano-graphite phase carbon nitride is 30-80nm.

4. The method for preparing an antistatic polystyrene material according to claim 1, Features: The rotation speed of the high-speed stirring is 350-450 rpm.

5. The method for preparing an antistatic polystyrene material according to claim 1, It is characterized in that The electrospinning parameters are as follows: the spinning temperature is 22-28° C., the spinning voltage is 14-15 kV, the relative humidity is 40-50%, the receiving distance between the receiving plate and the electrospinning nozzle device is 10-12 cm, and the spinning solution flow rate is 1.0-1.5 mL / h.

6. The method for preparing an antistatic polystyrene material according to claim 5, It is characterized in that The inner diameter of the electrospinning nozzle is 0.5-0.86 mm.

7. An antistatic polystyrene material prepared by the preparation method according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Synthesis method for porous graphite phase carbon nitride

    CN104843658A

  • Flame-retardant modified PMMA (polymethylmethacrylate) microspheres and preparation method thereof

    CN107522885A

  • Preparation method of hollow carbon spheres

    CN110482521A

  • Process for integrating preparation and loading of catalyst layer in oxygen cathode membrane electrode

    CN113394438A

  • Preparation method of polyacrylate hydrogel film

    CN115566265A