Solar cell and method for manufacturing the same
By designing the doping structure and process flow of the P and N regions on the back of the solar cell, more efficient carrier collection and electrode contact are achieved, which solves the problem of improving cell efficiency and improves light conversion efficiency and cell performance.
Patent Information
- Application Number
- CN202410917310.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-10
AI Technical Summary
The cell efficiency of existing solar cells has not yet reached its optimal state, especially in terms of carrier collection in the back P and N regions. There is room for improvement.
A solar cell design is adopted, in which the P region on the back includes a heavily doped region and a lightly doped region, the N region is provided with a tunneling layer and an N-type doped polysilicon layer, and the first electrode and the second electrode are both located on the back. Optimize the structure and process flow of the P and N regions, including forming the boron diffusion layer, annealing, removing the mask layer and preparing electrodes to ensure efficient contact and isolation of the electrodes.
It improves the light conversion efficiency, open circuit voltage and short circuit current of the solar cell, improves the overall cell efficiency, and increases the light receiving area through no metal electrode shielding.
Smart Images

Figure CN118472062B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the photovoltaic field, and in particular to a solar cell and a preparation method thereof. Background Art
[0002] BC (Back Contact) cell, also known as full back electrode contact cell or full reverse electrode contact cell, is a new type of solar cell technology.
[0003] BC cells use a design different from traditional crystalline silicon photovoltaic cells. Its electrodes are all located on the back of the cell, and the front is completely exposed to sunlight, which improves the light absorption efficiency; it can also reduce the current transmission path, reduce resistance, and improve battery performance.
[0004] However, although BC batteries have obvious advantages over other battery technology routes, battery efficiency still needs to be improved.
[0005] In view of this, it is necessary to provide an improved solar cell and a preparation method thereof to solve the above technical problems. Summary of the invention
[0006] The present invention provides a solar cell and a preparation method thereof, which improves the carrier collection of the P region and the N region on the back side of the cell, thereby improving the cell efficiency.
[0007] In order to achieve one of the above-mentioned invention objects, the present invention adopts the following technical solution:
[0008] A solar cell, comprising:
[0009] A P region located at the back side, wherein the P region includes a heavily doped region and a lightly doped region;
[0010] An N region located at the back side, wherein the N region is provided with a tunneling layer and an N-type doped polysilicon layer;
[0011] A first electrode, located on the back side of the heavily doped region;
[0012] The second electrode is located on the back side of the N-type doped polysilicon layer.
[0013] In an optional implementation, the square resistance of the heavily doped region is 80 ohm / sq to 130 ohm / sq, and the square resistance of the lightly doped region is 200 ohm / sq to 400 ohm / sq.
[0014] In an optional implementation, the diffusion depth of the P region is greater than the diffusion depth of the N region.
[0015] In an optional implementation, the boron junction depth of the P region is 0.5 μm to 1.0 μm.
[0016] In an optional implementation, the doping concentration of the N region is less than the doping concentration of the N-type doped polysilicon layer.
[0017] In an optional implementation, the solar cell further includes an isolation region between the P region and the N region, and a width of the isolation region is no greater than 100 μm.
[0018] In an optional embodiment, the solar cell also includes: a back passivation layer and a back anti-reflection layer located on the back side, the first electrode passes through the back anti-reflection layer and the back passivation layer to contact the heavily doped region; the second electrode passes through the back anti-reflection layer and the back passivation layer to contact the N-type doped polysilicon layer; and a front passivation layer and a front anti-reflection layer are sequentially arranged on the front side of the silicon substrate.
[0019] A method for preparing a solar cell comprises the following steps:
[0020] A boron diffusion layer and BSG are formed on the back of the silicon substrate, wherein the gate line region of the P region is a heavily doped region, and the region outside the gate line region is a lightly doped region;
[0021] removing the BSG and the boron junction outside the P region;
[0022] forming a tunneling layer, an N-type doped amorphous silicon layer and a mask layer on the entire back side of the silicon substrate;
[0023] Annealing, the N-type doped amorphous silicon layer is transformed into an N-type doped polysilicon layer, and phosphorus diffuses into the silicon substrate to form an N-type doped region;
[0024] Removing the mask layer, the N-type doped polysilicon layer and the tunneling layer outside the N region spaced apart from the P region;
[0025] The first electrode and the second electrode are prepared in the P region and the N region respectively.
[0026] In an optional embodiment, "forming a boron diffusion layer and BSG" includes the following steps: forming a boron source on the entire back side of the silicon substrate; laser scanning in the gate line area of the P region to form a heavily doped area; sending the heavily doped silicon substrate into a tube furnace and introducing oxygen at a temperature of 950°C~1000°C and an oxygen flow rate of 10sml~15sml; forming a lightly doped area outside the gate line area, and simultaneously introducing oxygen to form a layer of BSG on the entire surface.
[0027] In an optional implementation, the square resistance of the heavily doped region is 80 ohm / sq to 130 ohm / sq, and the square resistance of the lightly doped region is 200 ohm / sq to 400 ohm / sq.
[0028] In an optional embodiment, “removing the BSG and the boron junction outside the P region” comprises the following steps:
[0029] Laser film opening to remove the BSG layer outside the P region;
[0030] The BSG on the front and side surfaces of the silicon substrate is removed by using an HF solution, the volume concentration of the HF solution being 5% to 20%;
[0031] Polishing is performed to remove the boron junction outside the P region and the boron junction expanded on the front side.
[0032] In an optional embodiment, the tunneling layer is SiOx with a thickness of 1.4 nm to 2.3 nm; or the tunneling layer is SiC with a thickness of 1 nm to 1.8 nm.
[0033] In an optional embodiment, the tunneling layer is silicon oxide, has a thickness of 1.4 nm to 2.3 nm, and an annealing temperature of 880° C. to 950° C.
[0034] In an optional embodiment, the tunneling layer is a silicon carbide layer with a thickness of 1 nm to 1.8 nm and an annealing temperature of 850° C. to 900° C.
[0035] In an optional embodiment, “removing the mask layer, the N-type doped polysilicon layer and the tunneling layer outside the N region spaced apart from the P region” comprises the following steps:
[0036] Laser film opening to remove the mask layer outside the N region;
[0037] A chain machine is used to remove the mask layer of the front side expansion;
[0038] A slot machine is used to remove the N-type doped polysilicon layer and tunneling layer outside the N region on the back side, and at the same time a pyramid structure is formed on the front side of the silicon substrate.
[0039] In an optional embodiment, before preparing the first electrode and the second electrode, the method for preparing a solar cell further includes the following steps:
[0040] Depositing a passivation layer on the front and back sides, wherein the passivation layer is an aluminum oxide layer with a thickness of 3nm to 6nm;
[0041] An anti-reflection layer is deposited on the front and back sides, and the anti-reflection layer is selected from a laminated film of one or more of silicon nitride, silicon oxynitride, and silicon oxide, and the thickness of the anti-reflection layer is 60nm~130nm.
[0042] In an optional embodiment, after the first electrode and the second electrode are prepared, the first electrode and the second electrode are laser sintered using a laser-assisted sintering technique.
[0043] In an optional embodiment, the laser wavelength is 1064 nm or 532 nm, and the laser width is 100 microns or 1 mm to 2 mm.
[0044] The beneficial effects of the present invention are as follows: the solar cell of the present invention has a large light receiving area and high light conversion efficiency by arranging both the first electrode and the second electrode on the back side, and there is no metal electrode blocking the front side, thereby improving the cell efficiency. The SE structure is arranged in the P region, thereby improving the open circuit voltage and short circuit current of the cell; the passivation contact structure is arranged in the N region, and the surface is passivated, thereby improving the short circuit current and improving the cell efficiency as a whole. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 is a schematic structural diagram of a solar cell in one embodiment of the present invention;
[0046] Figure 2 The present invention is a flow chart of a method for preparing a solar cell according to an embodiment of the present invention.
[0047] Among them, 100-solar cell, 1-silicon substrate, 2-P region, 21-heavily doped region, 22-lightly doped region, 3-N region, 31-tunneling layer, 32-N-type doped polysilicon layer, 4-isolation region, 5-back passivation layer, 6-back anti-reflection layer, 7-front passivation layer, 8-front anti-reflection layer, 91-first electrode, 92-second electrode. DETAILED DESCRIPTION
[0048] The present invention will be described in detail below in conjunction with the specific embodiments shown in the accompanying drawings. However, these embodiments do not limit the present invention, and any structural, methodological, or functional changes made by a person skilled in the art based on these embodiments are all within the scope of protection of the present invention.
[0049] In the various drawings of the present invention, for the convenience of illustration, some sizes of structures or parts are exaggerated relative to other structures or parts, and thus, they are only used to illustrate the basic structure of the subject matter of the present invention.
[0050] With the shortening of the BC battery process and the breakthrough of key manufacturing technology, the mass production process is also accelerating. In order to further improve the efficiency of solar cells, the present invention optimizes the structure on the back of the battery, optimizes the N area and P area through different processes, and comprehensively improves the battery efficiency.
[0051] The present invention provides a solar cell 100 , which includes a silicon substrate 1 , a P region 2 and an N region 3 on the back of the silicon substrate 1 , a first electrode 91 on the back of the P region 2 , and a second electrode 92 on the back of the N region 3 .
[0052] The solar cell 100 has the first electrode 91 and the second electrode 92 disposed on the back side, and the front side is not blocked by metal electrodes, so the light receiving area is large, thereby improving the cell efficiency.
[0053] The silicon substrate 1 is an N-type silicon wafer with a resistivity of 0.3Ω·cm to 7Ω·cm, preferably 0.5Ω·cm to 3.5Ω·cm. In an optional embodiment, the front surface of the silicon substrate 1 has a suede structure, which has a good light limiting effect and can further improve the utilization rate of light.
[0054] The P region 2 and the N region 3 are arranged alternately, and an isolation region 4 is provided between the P region 2 and the N region 3. The isolation region 4 completely isolates the P region 2 and the N region 3 to avoid leakage problems caused by contact between the two. In the present invention, the width of the isolation region 4 is not greater than 100 μm, preferably 10 μm to 80 μm; on the premise that the P region 2 and the N region 3 can be effectively isolated, the width of the isolation region 4 is as small as possible.
[0055] The P region 2 includes a plurality of first main gate regions extending along a first direction and a plurality of first auxiliary gate regions extending along a second direction. The plurality of first auxiliary gate regions are arranged along the first direction, and the first auxiliary gate regions are connected to the first main gate regions.
[0056] In an optional embodiment, the P region 2 includes a heavily doped region 21 and a lightly doped region 22 to form a selective emitter to reduce surface recombination.
[0057] The first electrode 91 is located in the heavily doped region 21. Specifically, the first electrode 91 includes a first main gate and a first sub-gate, wherein the width of the first main gate is smaller than the width of the first main gate region, and the first main gate is located in the gate line region of the first main gate region; the width of the first sub-gate is smaller than the width of the first sub-gate region, and the first sub-gate is located in the gate line region of the first sub-gate region.
[0058] The gate line region is a heavily doped region 21, which forms an ohmic contact with the first electrode 91, reduces the series resistance of the battery, and improves the fill factor FF of the battery; and the non-gate line region outside the gate line region is a lightly doped region 22, which reduces the probability of carrier surface recombination and reduces the reverse saturation current of the battery, thereby increasing the open circuit voltage Voc and short circuit current Isc of the battery. In addition, the heavily doped region 21 and the lightly doped region 22 can generate a P++ / P+ high-low junction in the lateral direction, which is conducive to improving the collection of carriers and further increasing the short circuit current Isc.
[0059] In an optional embodiment, the doping concentration of the heavily doped region 21 is 5E18cm -3 ~1E20cm -3 , the square resistance is 80ohm / sq~130ohm / sq, and the square resistance of the lightly doped region 22 is 200ohm / sq~400ohm / sq.
[0060] In the present invention, the diffusion depth of the P region 2 is greater than the diffusion depth of the N region 3. In an optional embodiment, the boron junction depth of the P region 2 is 0.5 μm to 1.0 μm. At this time, the P region 2 and the N region 3 reach the optimal passivation level, and the dark saturation current density J0 of the P region 2 is 2 to 4 fA / cm 2 , the dark saturation current density J0 of N region 3 is between 1 and 3 fA / cm 2 , when this optimum passivation level is reached, a more or less fixed junction depth level occurs.
[0061] The N region 3 includes a plurality of second main gate regions extending along the first direction and a plurality of second sub-gate regions extending along the second direction, wherein the plurality of second sub-gate regions are arranged along the second direction, and the second sub-gate regions are connected to the second main gate regions. The first main gate regions and the second main gate regions are alternately arranged along the second direction, and the first sub-gate regions and the second sub-gate regions are alternately arranged along the first direction, so that the P region 2 and the N region 3 are arranged in a forked shape as a whole.
[0062] The present invention optimizes the N region 3 in combination with the TOPCon battery technology, and arranges a tunneling layer 31 and an N-type doped polysilicon layer 32 on the back side of the N region 3 to form a passivation contact structure. The second electrode 92 is located on the back side of the N-type doped polysilicon layer 32 to avoid direct contact between the second electrode 92 and the silicon substrate 1, thereby improving the battery efficiency.
[0063] The tunneling layer 31 is selected from a silicon oxide layer (SiOx) or a silicon carbide layer (SiC), and has a thickness of 1nm to 3nm, preferably 1nm to 2.5nm, and more preferably 1nm to 2nm or 1.5nm to 2.5nm. The present invention optimizes the thickness according to the density of the tunneling layer 31. When the tunneling layer 31 is SiOx, the thickness is between 1.4nm and 2.3nm; when the tunneling layer 31 is SiC, the film layer is more dense, and the thickness is 1nm to 1.8nm.
[0064] The N-type doped polysilicon layer 32 is a phosphorus-doped polysilicon layer, a carbon-doped polysilicon layer, or a nitrogen-doped polysilicon layer. Phosphorus-doping is used as an example for the following description. The doping concentration is 1E19 cm -3 ~1E21cm -3 , preferably 1E20cm -3 ~9E20cm -3 ; The thickness is 80nm~120nm, and can be set to 90nm, or 85nm, or 100nm, or 105nm, or 110nm, or 115nm.
[0065] In the present invention, the doping concentration of the N region 3 is less than the doping concentration of the N-type doped polysilicon layer 32. Based on this design, when the phosphorus-doped amorphous silicon layer is annealed and converted into the N-type doped polysilicon layer 32, phosphorus diffuses inward, passes through the tunneling layer 31 and enters the silicon substrate 1 to form the N region 3; there is no need to diffuse phosphorus in the N region 3 separately.
[0066] In an optional embodiment, the doping concentration of the N region 3 is 1E19 cm -3 ~1E20cm -3 The doping concentration of the N-type doped polysilicon layer 32 is 3E20cm -3 ~6E20cm -3 .
[0067] In addition, the back side of the solar cell 100 is also provided with a back side passivation layer 5 and a back side anti-reflection layer 6, and the first electrode 91 passes through the back side anti-reflection layer 6 and the back side passivation layer 5 to contact the heavily doped region 21; the second electrode 92 passes through the back side anti-reflection layer 6 and the back side passivation layer 5 to contact the N-type doped polysilicon layer 32.
[0068] The back passivation layer 5 is preferably an aluminum oxide layer, which provides excellent field passivation effect for the P region 2 and excellent interface passivation effect for the N region 3. In the present invention, the thickness of the back passivation layer 5 is preferably 3nm to 6nm.
[0069] The back anti-reflection layer 6 is selected from one or more laminated films of silicon nitride, silicon oxynitride, and silicon oxide, with a thickness of 60nm to 130nm, which reduces reflectivity and improves light utilization.
[0070] In an optional embodiment, the solar cell 100 further includes a front passivation layer 7 and a front anti-reflection layer 8 sequentially disposed on the front side of the silicon substrate 1 to passivate the surface defects on the front side. In the present invention, the material and thickness of the front passivation layer 7 and the back passivation layer 5 are consistent, and the two can be deposited together; the material and thickness of the front anti-reflection layer 8 and the back anti-reflection layer 6 are consistent, and the two can also be deposited in the same process.
[0071] The present invention also provides a method for preparing a solar cell, comprising the following steps:
[0072] A boron diffusion layer and BSG (borosilicate glass) are formed on the back of the silicon substrate 1, wherein the gate line region of the P region 2 is a heavily doped region 21, and the region outside the gate line region is a lightly doped region 22;
[0073] Removing the BSG and the boron junction outside the P region 2;
[0074] The entire back surface is deposited with a tunneling layer 31, a phosphorus-doped amorphous silicon layer and a mask layer;
[0075] Annealing, the doped amorphous silicon layer is transformed into an N-type doped polysilicon layer 32, and phosphorus diffuses into the silicon substrate 1 to form a phosphorus doped region;
[0076] The mask layer, the N-type doped polysilicon layer 32 and the tunneling layer 31 outside the N region 3 spaced apart from the P region 2 are removed;
[0077] A first electrode 91 and a second electrode 92 are prepared in the P region 2 and the N region 3 respectively.
[0078] For the convenience of description, the method for preparing the solar cell of the present invention is described in detail below.
[0079] S1 forms a boron diffusion layer and BSG on the back side of the silicon substrate 1, wherein the boron diffusion layer is an SE structure, the gate line region of the P region 2 is a heavily doped region 21, and other regions outside the gate line region of the P region 2 are lightly doped regions 22. Specifically, the following steps are included:
[0080] S11 first forms a boron source on the entire back side of the silicon substrate 1. In an optional implementation, the silicon substrate 1 is fixed in a quartz boat, sent into a tube furnace, and a boron source and oxygen are introduced to deposit a layer of boron source (or referred to as a through source) on the back side of the silicon substrate 1. Wherein, the boron source is boron trichloride (BCl3), the flow rate of boron trichloride is 90sccm~150sccm, the flow rate of oxygen reacting with BCl3 is 100sccm~500sccm, and the flow rate of oxygen used to generate an oxide layer is 1slm~10slm; or, the boron source is boron tribromide (BBr3), the flow rate of boron trichloride is 90sccm~150sccm, the flow rate of oxygen reacting with BBr3 is 100sccm~500sccm, and the flow rate of oxygen used to generate an oxide layer is 1slm~10slm.
[0081] S12 laser processing to form a heavily doped region 21. Specifically, laser scanning is performed in the gate line region of the P region 2 to form the heavily doped region 21. Laser parameters: laser gas power is 120W, 63% power is used for wafer processing; laser frequency is 100kHZ, and scanning speed is 25m / s.
[0082] S13 forms a lightly doped region 22 outside the gate line region, and simultaneously oxidizes the entire surface to form a BSG layer.
[0083] In an optional embodiment, the heavily doped silicon substrate 1 is placed in a tube furnace, and oxygen is introduced into the tube furnace at a temperature of 950°C~1000°C and an oxygen flow rate of 10sml~15sml; under high temperature, the boron source in the non-gate line area diffuses inward to form a lightly doped area 22, and BSG is formed on the entire surface.
[0084] In an optional embodiment, the sheet resistance after depositing the boron source is 120 ohm / sq~170 ohm / sq; after laser scanning, the doping concentration of the heavily doped region 21 is 5E18 cm -3 ~1E20cm -3 , the square resistance is 80ohm / sq~130ohm / sq; after high-temperature oxidation, the square resistance of the lightly doped region 22 is 200ohm / sq~400ohm / sq.
[0085] S2 "removing the BSG and boron junction outside the P region 2" includes the following steps:
[0086] S21 removes the BSG outside the P region 2. Optionally, laser film opening is performed outside the P region 2 to remove the BSG layer, with a laser power of 50W to 120W, preferably ultraviolet picosecond or green picosecond laser, which has low damage and low cost; femtosecond laser can also be used.
[0087] S22 removes the boron junction outside the P region 2. Specifically, it includes the following steps:
[0088] First, the BSG on the front and side surfaces of the silicon substrate 1 is removed by HF solution, the concentration of the HF solution being 5% to 20% (volume concentration). In an optional embodiment, this step is completed in a chain machine.
[0089] Polishing is then performed to remove the boron junction outside the P region 2 and the boron junction on the front side, while the boron junction and BSG in the P region 2 are retained. In an optional embodiment, this step is completed in a slot machine.
[0090] This step removes the boron junction outside the P region 2 while removing the BSG on the front and side surfaces and the boron junction expanded on the front side. The process is simple and lays a good foundation for subsequent process preparation.
[0091] S3 “depositing a tunneling layer 31, a doped amorphous silicon layer and a mask layer on the back side” includes: growing a tunneling layer 31 and a phosphorus-doped amorphous silicon layer on the entire back side by PECVD in-situ doping, and then growing a mask layer on the outermost side.
[0092] In one embodiment, the tunneling layer 31 is SiOx, and the thickness is preferably 1.4 nm to 2.3 nm.
[0093] In another embodiment, the tunneling layer 31 is SiC, which is denser and preferably has a thickness of 1 nm to 1.8 nm.
[0094] The thickness of the N-poly layer is preferably 80 nm to 120 nm.
[0095] The mask layer is preferably a silicon oxide layer, and the thickness is controlled within the range of 10nm to 50nm.
[0096] S4 uses a high temperature annealing furnace, and the annealing temperature can be matched according to the tunneling conditions. The thickness of the tunneling layer 31 is large, and the annealing temperature is high. In an optional embodiment, the annealing temperature is 850℃~950℃, which can match the conventional tunneling layer 31 at a better level and ensure the doping concentration of 1E19cm in the electrochemical doping concentration test (ECV test) of the n-poly region. -3 ~1E21cm -3 .
[0097] In this process, a BSG layer is retained in the tunneling layer 31 of the P region 2 to hinder the inward diffusion of phosphorus; while outside the P region 2, phosphorus diffuses through the tunneling layer 31 to the silicon substrate 1 to form a phosphorus-doped region.
[0098] The annealing temperature is related to the density and thickness of the tunneling layer 31. In an optional embodiment, when the tunneling layer 31 is silicon oxide, the thickness is 1.4nm~2.3nm, and the annealing temperature is 880℃~950℃; when the tunneling layer 31 is a silicon carbide layer, the thickness is 1nm~1.8nm, and the annealing temperature is 850℃~900℃; to ensure that phosphorus outside the P region 2 diffuses inward to the silicon substrate 1.
[0099] S5 “removing the mask layer, the N-type doped polysilicon layer 32 and the tunneling layer 31 outside the N region 3 spaced apart from the P region 2” includes the following steps:
[0100] S51 uses a laser process to remove the mask layer outside the N region 3 to expose the N-type doped polysilicon layer 32 below. Laser parameters: laser power 50W~120W, preferably ultraviolet picosecond or green picosecond laser, the laser with less damage is more conducive to film opening.
[0101] S52 uses a chain machine and HF solution to remove the mask layer of the front side expansion.
[0102] S53 uses a slot machine and alkaline solution to remove the N-type doped polysilicon layer 32 and the tunneling layer 31 outside the back N region 3; at the same time, the front side of the silicon substrate 1 is etched with alkaline solution to form a pyramid structure on the exposed silicon substrate 1, and then cleaned.
[0103] Compared with the related art of "first forming a velvet structure on the surface of the silicon substrate 1 and then preparing other film layers", the present invention forms the pyramid structure on the front side after the important structures and film layers of the P region 2 and the N region 3 are prepared. On the one hand, there is no need to polish the back side before boron diffusion; on the other hand, step S53 forms the pyramid structure on the front side while removing the N-type doped polysilicon layer 32 and the tunneling layer 31 on the back side, thus achieving multiple goals at one stroke; furthermore, when the front side is a flat surface, it is more conducive to the deposition and cleaning of the film layers in the above steps.
[0104] In addition, the boron junction, tunneling layer 31, and N-type doped polysilicon layer 32 between the P region 2 and the N region 3 have been removed to form an isolation region 4 to prevent leakage between the P region 2 and the N region 3. In the present invention, the width of the isolation region 4 is not greater than 100 μm, preferably 10 μm to 80 μm. Under the premise of isolating leakage, the narrower the width of the isolation region 4, the smaller the recombination of carriers in this region, and the higher the battery efficiency.
[0105] S6 Double-sided passivation. Aluminum oxide is deposited on the front and back sides using the ALD process, with a thickness of preferably 3nm to 6nm. Al2O3 provides excellent field passivation effect for the P region 2 and excellent interface passivation effect for the N region 3. In the present invention, the double-sided passivation layer is an optional process step.
[0106] S7 double-sided anti-reflection layer: can be a laminated film composed of one or more of silicon nitride, silicon oxynitride, and silicon oxide, and the thickness of the anti-reflection layer is 60nm~130nm. In the present invention, the double-sided anti-reflection layer is an optional process step.
[0107] S8 electrode preparation: The electrodes are prepared by screen printing + sintering, including the preparation of the main gate electrode on the back side and the preparation of the secondary gate electrodes on the back side P region 2 and N region 3.
[0108] S9 uses laser-assisted sintering technology (Laser-enhanced contact optimization, LECO technology, also known as laser enhanced contact optimization) to laser sinter the first electrode 91 and the second electrode 92, which can improve the contact between silver and silicon in the electrode, thereby increasing the battery efficiency by more than 0.2%~0.3%; it can also change the electrode slurry, use silver-copper slurry with low silver content, etc., to save costs.
[0109] The laser wavelength is 1064nm or 532nm, and the laser width is 100 microns or 1mm~2mm.
[0110] In summary, the solar cell 100 of the present invention has a large light receiving area and high light conversion efficiency by setting the first electrode 91 and the second electrode 92 on the back side, without metal electrode blocking the front side, thereby improving the cell efficiency. The SE structure is set in the P region 2 to improve the open circuit voltage and short circuit current of the cell; the passivation contact structure is set in the N region 3 to passivate its surface, thereby improving the short circuit current and improving the cell efficiency as a whole.
[0111] It should be understood that although this specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each implementation mode may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
[0112] The series of detailed descriptions listed above are only specific descriptions of feasible implementation methods of the present invention. They are not intended to limit the scope of protection of the present invention. Any equivalent implementation methods or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.
Claims
1. A solar cell, characterized in that: include: A P region located at the back, the P region includes a heavily doped region and a lightly doped region; the P region is a boron diffusion layer formed by boron directly diffusing inward from the back of the silicon substrate; the boron junction depth of the P region is 0.5 μm to 1.0 μm; An N region located at the back side, wherein the N region is provided with a tunneling layer and an N-type doped polysilicon layer; A first electrode, located on the back side of the heavily doped region; The second electrode is located on the back side of the N-type doped polysilicon layer.
2. The solar cell according to claim 1, characterized in that: The square resistance of the heavily doped region is 80 ohm / sq to 130 ohm / sq, and the square resistance of the lightly doped region is 200 ohm / sq to 400 ohm / sq.
3. The solar cell according to claim 1, characterized in that: The diffusion depth of the P region is greater than the diffusion depth of the N region.
4. The solar cell according to claim 1, characterized in that: The doping concentration of the N region is lower than the doping concentration of the N-type doped polysilicon layer.
5. The solar cell according to claim 1, characterized in that: The solar cell further includes an isolation region between the P region and the N region, and a width of the isolation region is no greater than 100 μm.
6. The solar cell according to claim 1, characterized in that: The solar cell further comprises: A back passivation layer and a back anti-reflection layer are located on the back side, the first electrode passes through the back anti-reflection layer and the back passivation layer to contact the heavily doped region; the second electrode passes through the back anti-reflection layer and the back passivation layer to contact the N-type doped polysilicon layer; A front passivation layer and a front anti-reflection layer are sequentially arranged on the front side of the silicon substrate.
7. A method for preparing a solar cell, characterized in that: The steps include: A boron diffusion layer and BSG are formed on the back of the silicon substrate, wherein the gate line region of the P region is a heavily doped region, and the region outside the gate line region is a lightly doped region; boron is directly diffused inward on the back of the silicon substrate to form the boron diffusion layer; removing the BSG and the boron junction outside the P region; forming a tunneling layer, an N-type doped amorphous silicon layer and a mask layer on the entire back side of the silicon substrate; Annealing, the N-type doped amorphous silicon layer is transformed into an N-type doped polysilicon layer, and phosphorus diffuses into the silicon substrate to form an N-type doped region; Removing the mask layer, the N-type doped polysilicon layer and the tunneling layer outside the N region spaced apart from the P region; Prepare a first electrode and a second electrode in the P region and the N region respectively; Wherein, “removing the mask layer, the N-type doped polysilicon layer and the tunneling layer outside the N region spaced apart from the P region” includes the following steps: removing the mask layer outside the N region; Removing the mask layer of the front side expansion; The N-type doped polysilicon layer and the tunneling layer outside the back N region are removed, and a pyramid structure is formed on the front side of the silicon substrate.
8. The method for preparing a solar cell according to claim 7, characterized in that: "Forming a boron diffusion layer and BSG" includes the following steps: forming a boron source on the entire back side of the silicon substrate; Laser scanning is performed on the gate line region of the P region to form a heavily doped region; The heavily doped silicon substrate is sent into a tube furnace and oxygen is introduced at a temperature of 950℃~1000℃ and an oxygen flow rate of 10sml~15sml; a lightly doped area is formed outside the gate line area, and oxygen is introduced at the same time to form a layer of BSG on the entire surface.
9. The method for preparing a solar cell according to claim 8, characterized in that: The square resistance of the heavily doped region is 80 ohm / sq to 130 ohm / sq, and the square resistance of the lightly doped region is 200 ohm / sq to 400 ohm / sq.
10. The method for preparing a solar cell according to claim 7, characterized in that: "Removing BSG and boron junction outside the P region" includes the following steps: Laser film opening to remove the BSG layer outside the P region; The BSG on the front and side surfaces of the silicon substrate is removed by using an HF solution, the volume concentration of the HF solution being 5% to 20%; Polishing is performed to remove the boron junction outside the P region and the boron junction expanded on the front side.
11. The method for preparing a solar cell according to claim 7, characterized in that: The tunneling layer is SiOx with a thickness of 1.4nm-2.3nm; or the tunneling layer is SiC with a thickness of 1nm-1.8nm.
12. The method for preparing a solar cell according to claim 7, characterized in that: The tunneling layer is silicon oxide, has a thickness of 1.4 nm to 2.3 nm, and an annealing temperature of 880° C. to 950° C.; or The tunneling layer is a silicon carbide layer with a thickness of 1nm-1.8nm and an annealing temperature of 850°C-900°C.
13. The method for preparing a solar cell according to claim 7, characterized in that: “Removing the mask layer, the N-type doped polysilicon layer and the tunneling layer outside the N region spaced apart from the P region” comprises the following steps: Laser film opening to remove the mask layer outside the N region; Use chain machine and HF acid to remove the mask layer of the front side expansion; A trough machine and alkaline solution are used to remove the N-type doped polysilicon layer and tunneling layer outside the N region on the back side, and a pyramid structure is formed on the front side of the silicon substrate.
14. The method for preparing a solar cell according to claim 7, characterized in that: Before preparing the first electrode and the second electrode, the method for preparing a solar cell further comprises the following steps: Depositing a passivation layer on the front and back sides, wherein the passivation layer is an aluminum oxide layer with a thickness of 3nm to 6nm; An anti-reflection layer is deposited on the front and back sides, and the anti-reflection layer is selected from a laminated film of one or more of silicon nitride, silicon oxynitride, and silicon oxide, and the thickness of the anti-reflection layer is 60nm~130nm.
15. The method for preparing a solar cell according to any one of claims 7 to 14, characterized in that: After the first electrode and the second electrode are prepared, the first electrode and the second electrode are laser sintered by using a laser assisted sintering technology.
16. The method for preparing a solar cell according to claim 15, characterized in that: The laser wavelength is 1064nm or 532nm, and the laser width is 100 microns or 1mm~2mm.
Citation Information
Patent Citations
Efficient solar cell and preparation method thereof
CN112510105A
Solar cell and preparation method thereof