Composite positive electrode material and preparation method, positive electrode sheet, battery and electrical equipment

By adopting the structural design of composite cathode materials in battery materials, combined with high-speed mechanical fusion methods, conductive functional materials and insulating materials are placed in the holes of active materials, which solves the thermal stability and safety issues of battery materials and improves the performance of batteries. Electrical conductivity and cycle performance reduce the risk of internal short circuit.

CN118472228BActive Publication Date: 2024-10-29PHYLION BATTERY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410931769.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-29
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

While pursuing high energy density, existing battery materials often sacrifice safety and stability, especially insufficient thermal stability, which limits the application and safety of batteries in high-temperature environments.

Method used

A composite cathode material is used, including a first active material, a ternary material, a conductive functional material and an insulating material. The conductive functional material and the insulating material are placed in the first hole through a high-speed mechanical fusion method, and the ternary material is placed in the second hole. , forming a core-shell composite structure to improve electrical conductivity and thermal stability, and reduce the risk of internal short circuits through the high mechanical strength and heat resistance of insulating materials.

Benefits of technology

It improves the conductivity and thermal stability of the battery, reduces internal resistance, prevents thermal runaway, enhances the safety performance and cycle performance of the battery, and reduces the risk of acupuncture safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118472228B_ABST
    Figure CN118472228B_ABST
Patent Text Reader

Abstract

The present invention provides a composite positive electrode material and a preparation method, a positive electrode sheet, a battery and electrical equipment, belonging to the technical field of battery materials. The composite positive electrode material includes: a first active material, a ternary material, a conductive functional material and an insulating material; a first hole is provided on the surface of the first active material; a second hole is provided on the surface of the ternary material; the conductive functional material and the ternary material can both be placed in the first hole; the insulating material can be placed in the second hole. The composite positive electrode material provided by the present invention can improve the room temperature conductivity, reduce the internal resistance, and form an internal blockage to prevent thermal runaway through structural optimization, combining the ternary material and the conductive functional material; the high strength, stability and heat resistance of the insulating material can reduce the risk of internal short circuit and improve safety and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery materials, and in particular relates to a composite positive electrode material and a preparation method thereof, a positive electrode sheet, a battery and electrical equipment. Background Art

[0002] As a key component of modern energy storage, battery technology plays a vital role in electric vehicles, mobile devices, energy storage systems and other fields. With the transformation of the global energy structure and the growing demand for sustainable energy, the research and development of high-performance battery materials has become particularly urgent. The performance of battery materials directly affects the energy density, cycle stability, safety and cost-effectiveness of the battery, and is the core element that drives the advancement of battery technology.

[0003] Among the many battery materials, lithium manganese oxide, lithium iron manganese phosphate, lithium iron phosphate and ternary materials have attracted much attention due to their unique chemical properties and electrochemical performance. Lithium manganese oxide occupies a place in battery materials due to its good thermal stability and cycle performance, while lithium iron manganese phosphate and lithium iron phosphate are favored due to their high theoretical capacity and cost-effectiveness. However, these materials usually face the problem of insufficient energy density, which limits their application in high-performance batteries. In contrast, ternary materials are known for their high energy density, which can provide longer driving range and faster charging speed, but their lack of thermal stability has become the main obstacle to their widespread application.

[0004] The defects of the existing technology are mainly reflected in the comprehensive performance of battery materials. Although lithium manganese oxide has good stability, its low energy density limits its application in scenarios with high capacity requirements. Although lithium iron manganese phosphate and lithium iron phosphate have high theoretical capacity, they are often difficult to achieve the expected performance in practical applications, and their stability in high temperature environments is poor. Although ternary materials have advantages in energy density, their poor thermal stability and safety issues make the battery a potential safety hazard under extreme conditions, especially in fast charging or high temperature environments, the risk of thermal runaway of the battery is significantly increased.

[0005] On the whole, existing battery materials often sacrifice safety and stability while pursuing high energy density. This contradiction is particularly prominent in the selection of battery materials and battery design. The lack of thermal stability of battery materials, the balance between energy density and cycle stability, and cost-effectiveness considerations are all key issues that need to be urgently addressed in the current development of battery technology. The existence of these problems not only limits the application of battery technology in a wider range of fields, but also poses challenges to the long-term reliability and safety of batteries. Therefore, the development of a battery material that has both high energy density and good thermal stability and safety is of great significance to promoting the development of battery technology. Summary of the invention

[0006] In order to solve the above problems, the present invention provides a composite positive electrode material, comprising: a first active material, a ternary material, a conductive functional material and an insulating material;

[0007] The first active material has a first hole on its surface;

[0008] The surface of the ternary material is provided with a second hole;

[0009] The conductive functional material and the ternary material can both be placed in the first hole;

[0010] The insulating material can be placed in the second hole;

[0011] Preferably, the first active material, the ternary material, the conductive functional material and the insulating material satisfy the following relationship:

[0012] D 50(1) >D 1 >D 3 ≥D 50(2) >D 2 >D 4 ;

[0013] Among them, D 1 represents the diameter of the first hole; D 2 represents the diameter of the second hole; D 3 represents the diameter of the conductive functional material; D 4 Represents the diameter of the insulating material; D 50(1) D represents the first active material 50 ;D 50(2) D represents the ternary material 50 ;

[0014] Preferably, D of the first active material 50(1) The range is 10-50μm;

[0015] Preferably, D of the ternary material 50(2) The range is 0.1-5μm;

[0016] Preferably, D 1 The range is 1-10μm;

[0017] Preferably, D 2 The range is 50-200nm;

[0018] Preferably, D 3 The range is 1-10μm;

[0019] Preferably, D 4 The range is 10-100nm.

[0020] Preferably, the insulating material includes at least one of aluminum oxide, boehmite, silicon dioxide, zirconium dioxide, titanium dioxide, magnesium oxide, zinc oxide, and calcium oxide.

[0021] Preferably, the conductive functional material is a core-shell composite structure with a conductive material as the core and a thermosensitive polymer as the shell.

[0022] Preferably, the thermosensitive polymer comprises at least one of polyethylene, polypropylene, polyamide, polyesteramide, polystyrene, polyvinyl chloride, polyester, polyurethane, ethylene vinyl acetate polymer, ethylene acrylate polymer, olefin copolymer, propylene copolymer and ethylene copolymer.

[0023] Preferably, the conductive material includes at least one of polypyrrole, polythiophene, Ketjen black, conductive fiber, acetylene black, carbon nanotube, graphene, flake graphite, silicon carbide, molybdenum disilicide and lanthanum cobaltate.

[0024] Preferably, the composite positive electrode material further includes a second active material;

[0025] Preferably, the second active material includes at least one of an olivine-structured lithium manganese iron phosphate material, a layered lithium polyacid, a spinel-type lithium manganate, a layered manganese-rich lithium base, an olivine-type lithium iron phosphate and an olivine-type lithium manganese phosphate.

[0026] Preferably, the first active material includes at least one of an olivine-structured lithium manganese iron phosphate material, a layered polyacid lithium, a spinel-type lithium manganate, a layered manganese-rich lithium base, an olivine-type lithium iron phosphate and an olivine-type lithium manganese phosphate.

[0027] In addition, in order to solve the above problems, the present invention also provides a method for preparing the composite positive electrode material as described above, comprising:

[0028] The first active material, the ternary material, the conductive functional material and the insulating material are fused by a high-speed mechanical fusion method, so that the conductive functional material enters the first pores on the surface of the first active material, and the insulating material enters the second pores on the surface of the ternary material, to obtain the composite positive electrode material;

[0029] Preferably, the step of fusing the first active material, the ternary material, the conductive functional material and the insulating material by the high-speed mechanical fusion method also includes: adding a second active material so that the second active material and the conductive functional material can enter the first holes on the surface of the first active material by the high-speed mechanical fusion method.

[0030] In addition, in order to solve the above problems, the present invention also provides a positive electrode plate, including the composite positive electrode material as described above.

[0031] In addition, to solve the above problems, the present invention also provides a battery, including the positive electrode plate as described above.

[0032] In addition, in order to solve the above problems, the present invention also provides an electrical device, which uses the battery as described above.

[0033] The present invention provides a composite positive electrode material and a preparation method thereof, a positive electrode sheet, a battery and electrical equipment. The composite positive electrode material includes: a first active material, a ternary material, a conductive functional material and an insulating material; a first hole is provided on the surface of the first active material; a second hole is provided on the surface of the ternary material; both the conductive functional material and the ternary material can be placed in the first hole; the insulating material can be placed in the second hole. The composite positive electrode material provided by the present invention can overcome the shortcomings existing when the ternary material is used alone. By optimizing the material structure, the ternary material with poor thermal stability and the conductive functional material with conductivity are placed in the first active material through the first hole, thereby improving the conductive performance of the material at room temperature, effectively reducing the internal resistance of the battery, wrapping the ternary material, forming an internal blockage inside the battery, buffering and weakening the short-circuit current, and preventing the occurrence of further thermal runaway of the lithium-ion battery.

[0034] The insulating material has high mechanical strength, good stability and good heat resistance. It can protect the material well in the event of mechanical abuse of the battery (such as puncture, extrusion), further reducing or even avoiding internal short circuits, thereby improving the puncture safety of the battery, improving the safety performance of the battery, and can also enhance the high temperature resistance of the battery, stabilize the interface, improve the stability of the material, and improve the cycle performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 A schematic diagram of the structure of a composite positive electrode material in an embodiment of the present invention;

[0036] Figure 2 Schematic diagram of the structure of the composite positive electrode material (including the second active material) in an embodiment of the present invention;

[0037] Figure 3 This is a SEM electron microscope image of the composite positive electrode material in Example 1 of the present invention.

[0038] Reference numerals:

[0039] 100, composite positive electrode material; 1, first active material; 11, first pore; 2, ternary material; 21, second pore; 3, conductive functional material; 31, conductive material; 32, thermosensitive polymer; 4, insulating material; 5, second active material. DETAILED DESCRIPTION

[0040] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] refer to Figure 1 In an embodiment of the present application, a composite positive electrode material is provided, comprising: a first active material, a ternary material, a conductive functional material and an insulating material;

[0042] The first active material has a first hole on its surface;

[0043] The surface of the ternary material is provided with a second hole;

[0044] The conductive functional material and the ternary material can both be placed in the first hole;

[0045] The insulating material can be placed in the second hole;

[0046] The following table is derived from the above characteristics:

[0047] Table 1. Relationship between components in composite cathode materials

[0048]

[0049] From the above table, we can draw the following conclusions:

[0050] (1) The particle sizes of the ternary material, the conductive functional material and the insulating material are all smaller than the first active material;

[0051] (2) The ternary material, the conductive functional material and the insulating material can all be placed in the first hole;

[0052] (3) Insulating material particles can be placed in the second holes.

[0053] Therefore, the composite positive electrode material that has completed the "composite" treatment can have the following two structures:

[0054] Structure 1: The first active material has a first hole on its surface, and the first hole contains a ternary material, a conductive functional material, and an insulating material; and the second hole of the ternary material also contains an insulating material;

[0055] Structure 2: There is a first hole on the surface of the first active material, and the first hole contains a ternary material and a conductive functional material; and there is also an insulating material in the second hole of the ternary material.

[0056] It should be noted that the conductive functional material is a functional material having conductivity.

[0057] In summary, the composite positive electrode material provided in the embodiment of the present application can overcome the shortcomings of the ternary material when it is used alone. By optimizing the material structure, the ternary material with poor thermal stability and the conductive functional material with conductivity are placed in the first active material through the first hole, which improves the conductivity of the material at room temperature, can effectively reduce the internal resistance of the battery, and when the operating temperature of the battery reaches the thermosensitive temperature and above, the conductive functional material will melt to form multiple continuous electronic barrier layers, forming an internal block inside the battery, wrapping the ternary material, preventing the lithium ion battery from further thermal runaway, and improving the pass rate of the secondary battery in the puncture test, thermal runaway test, drop test, and high temperature test. The insulating material has high mechanical strength, good stability, and good heat resistance. It can protect the material well in the case of mechanical abuse of the battery (such as needle puncture, extrusion), further reduce or even avoid the occurrence of internal short circuit, thereby improving the needle puncture safety of the battery, improving the safety performance of the battery, and can also enhance the high temperature resistance of the battery, stabilize the interface, improve the stability of the material, and improve the cycle performance of the battery.

[0058] Furthermore, the first active material, the ternary material, the conductive functional material and the insulating material satisfy the following relationship:

[0059] D 50(1) >D 1 >D 3 ≥D 50(2) >D 2 >D 4 ;

[0060] Among them, D 1 represents the diameter of the first hole; D 2 represents the diameter of the second hole; D 3 represents the diameter of the conductive functional material; D 4 Represents the diameter of the insulating material; D 50(1) D represents the first active material 50 ;D 50(2) D represents the ternary material 50 ;

[0061] It can be seen from the above relationship that the particle size of the first active material can be the largest, and the first pores therein can accommodate a certain volume of the ternary material, the conductive functional material and the insulating material.

[0062] Furthermore, the second hole of the ternary material can also accommodate an insulating material of a certain volume.

[0063] It should be noted that the D 50, also known as the median diameter or the 50% point of the particle size distribution, is a statistical parameter of the particle size distribution. It indicates that among a series of particles of different sizes, half of the particles have a diameter less than D 50 value, the other half of the particles have a diameter larger than D 50 Value. 50 It is the median of the particle size distribution and is often used to describe the typical size or average particle size of particles. 50 is an important indicator because it provides intuitive information about the average size of the particle population.

[0064] Furthermore, D of the first active material 50(1) The range is 10-50μm;

[0065] Furthermore, the D of the ternary material 50(2) The range is 0.1-5μm;

[0066] Furthermore, D 1 The range is 1-10μm;

[0067] Furthermore, D 2 The range is 50-200nm;

[0068] Furthermore, D 3 The range is 1-10μm;

[0069] Furthermore, D 4 The range is 10-100nm.

[0070] Furthermore, the insulating material includes at least one of aluminum oxide, boehmite, silicon dioxide, zirconium dioxide, titanium dioxide, magnesium oxide, zinc oxide, and calcium oxide.

[0071] Furthermore, the conductive functional material is a core-shell composite structure with a conductive material as the core and a thermosensitive polymer as the shell.

[0072] Furthermore, the thermosensitive polymer includes at least one of polyethylene, polypropylene, polyamide, polyesteramide, polystyrene, polyvinyl chloride, polyester, polyurethane, ethylene vinyl acetate polymer, ethylene acrylate polymer, olefin copolymer, propylene copolymer and ethylene copolymer.

[0073] Furthermore, the conductive material includes at least one of polypyrrole, polythiophene, Ketjen black, conductive fiber, acetylene black, carbon nanotubes, graphene, flake graphite, silicon carbide, molybdenum disilicide and lanthanum cobaltate.

[0074] As mentioned above, the conductive functional material is a core-shell composite structure, wherein the conductive material is the core and the thermosensitive polymer is the shell.

[0075] The conductive functional material mentioned above is to solve the problem of poor thermal stability of ternary materials. Although ternary materials have high capacity, they have poor thermal stability and are prone to thermal runaway at high temperatures. By combining ternary materials with conductive functional materials, the thermosensitive properties of functional materials can be used to form an electron blocking layer at high temperatures, thereby improving the safety of the battery.

[0076] The core-shell structure design of the conductive functional material enables the conductive material and the thermosensitive polymer to work synergistically, which not only ensures the conductive performance of the battery but also improves the thermal stability and safety of the battery.

[0077] Conductive materials in conductive functional materials (such as polypyrrole, polythiophene, Ketjen black, etc.) can improve the conductivity of the material at room temperature, thereby effectively reducing the internal resistance of the battery.

[0078] The thermosensitive polymer will melt when the battery reaches a certain temperature, forming a continuous electron blocking layer, which helps to form a blockade inside the battery, buffering and weakening the short-circuit current.

[0079] When the battery temperature rises, the morphology and structure of the conductive functional material changes, wrapping the ternary material to prevent further thermal runaway of the lithium-ion battery. The conductive functional material can provide protection when the battery experiences thermal runaway and reduce safety risks.

[0080] In summary, the use of conductive functional materials is to improve the conductivity and safety of the battery, especially under high temperature conditions, to prevent thermal runaway of the battery through a thermosensitive response mechanism, thereby improving the overall performance and reliability of the battery.

[0081] Furthermore, the composite positive electrode material also includes a second active material;

[0082] Please refer to Figure 2 , which is an implementation method in the embodiments of the present application.

[0083] Furthermore, the second active material includes at least one of an olivine-structured lithium manganese iron phosphate material, a layered polyacid lithium, a spinel-type lithium manganese oxide, a layered manganese-rich lithium base, an olivine-type lithium iron phosphate and an olivine-type lithium manganese phosphate.

[0084] Furthermore, the first active material includes at least one of an olivine-structured lithium manganese iron phosphate material, a layered polyacid lithium, a spinel-type lithium manganese oxide, a layered manganese-rich lithium base, an olivine-type lithium iron phosphate and an olivine-type lithium manganese phosphate.

[0085] As mentioned above, the second active material is used together with the first active material to form a composite positive electrode material to improve the overall performance of the battery.

[0086] Among them, the second active material can enter the pores of the first active material together with the functional material through high-speed mechanical fusion. This structural design helps to improve the overall performance of the material.

[0087] The addition of a second active material can increase the energy density of the battery because the second active material may have a higher theoretical capacity or voltage platform, which helps to increase the total energy output of the battery.

[0088] The second active material has the characteristics of improving the charge and discharge performance of the battery, such as improving the cycle stability, reducing the polarization during the charge and discharge process, etc.

[0089] The second active material helps to improve the structural stability of the positive electrode material, especially during the charge and discharge process, reducing the volume expansion and structural degradation of the material.

[0090] The second active material helps improve the thermal stability and safety of the battery, especially under extreme conditions such as high temperature or overcharging.

[0091] In addition, an embodiment of the present application also provides a method for preparing the composite positive electrode material as described above, comprising:

[0092] The first active material, the ternary material, the conductive functional material and the insulating material are fused by a high-speed mechanical fusion method, so that the conductive functional material enters the first pores on the surface of the first active material, and the insulating material enters the second pores on the surface of the ternary material, to obtain the composite positive electrode material;

[0093] Furthermore, in the step of fusing the first active material, the ternary material, the conductive functional material and the insulating material by the high-speed mechanical fusion method, it also includes: adding a second active material so that the second active material and the conductive functional material can enter the first holes on the surface of the first active material by the high-speed mechanical fusion method.

[0094] As mentioned above, high-speed mechanical fusion is an industrial mixing technology that involves the use of a high-speed rotating mechanical device to mix different materials. This method is used to prepare composite materials to ensure uniform distribution and good interface bonding between the components. This method can effectively mix the first active material, the second active material, the functional material and the insulating material uniformly through high-speed mechanical fusion, ensuring good contact and interface bonding between the materials.

[0095] By introducing the second active material into the pores of the first active material together with the functional material, and the insulating material into the second pores, the material structure is optimized, which helps to improve the overall performance of the battery.

[0096] The core-shell structure design of the conductive functional material makes the conductive material the core and the thermosensitive polymer the shell. This structure helps to improve the conductive performance of the material at room temperature and reduce the internal resistance of the battery. The conductive functional material will melt at high temperature to form an electron barrier layer, which wraps the ternary material and prevents the battery from further thermal runaway, thereby improving the thermal stability and safety of the battery.

[0097] The addition of the insulating material, due to its high mechanical strength, stability and heat resistance, can provide protection when the battery suffers mechanical abuse, reduce the risk of internal short circuit, and improve the safety of the battery. Moreover, the addition of the insulating material helps to stabilize the interface of the battery material, improve the stability of the material, and thus enhance the cycling performance of the battery.

[0098] The above preparation method allows for the selection of different active materials, functional materials and insulating materials according to different application requirements, providing flexibility in material design.

[0099] In addition, an anode electrode sheet is provided in the embodiments of the present application, which includes the composite anode material as described above.

[0100] In addition, a battery is provided in the embodiments of the present application, which includes the anode electrode sheet as described above.

[0101] In addition, an electric device is provided in the embodiments of the present application, which uses the battery as described above.

[0102] The electric device may include, for example, but not limited to, smart mobile devices, wearable devices, household appliances, electric bicycles, electric vehicles, and the like.

[0103] The present invention will be further described below through specific embodiments. However, it should be understood that these embodiments are only used for more detailed description and should not be construed as limiting the present invention in any form.

[0104] Table 2. Sizes of each component in the embodiments

[0105]

[0106] In the above table, "Emb." represents an embodiment. For example, "Emb. 1" represents Embodiment 1, and so on.

[0107] Table 3. Sizes of each component in the comparative examples

[0108]

[0109] In the above table, "Comp." represents a comparative example. For example, "Comp. 1" represents Comparative Example 1, and so on.

[0110] Table 4. Components in the embodiments and comparative examples

[0111]

[0112] Embodiment 1:

[0113] In this embodiment, a composite positive electrode material was prepared by the following method. The parameters of each component in the preparation are shown in Table 2 and Table 4.

[0114] Experimental method: The particle size D 50(1) The particle size D is 20 μm. 50(2) The ternary material (NCM811) is 3μm, and the diameter D 3 The conductive functional material (graphene coated polyethylene) is 5 μm in diameter. 4 Alumina with a thickness of 50nm is fused mechanically at high speed to form a composite positive electrode material.

[0115] Among them, the first hole D 1 The second hole D is 8μm. 2 is 100nm.

[0116] The composite positive electrode material prepared in Example 1 was tested by SEM electron microscope. Figure 3 .

[0117] Embodiment 2:

[0118] In this embodiment, a composite positive electrode material was prepared by the following method. The parameters of each component in the preparation are shown in Table 2 and Table 4.

[0119] Experimental method: basically the same as Example 1, except that lithium manganese iron phosphate is replaced by lithium manganese oxide.

[0120] Embodiment 3:

[0121] In this embodiment, a composite positive electrode material was prepared by the following method. The parameters of each component in the preparation are shown in Table 2 and Table 4.

[0122] Experimental method: basically the same as Example 1, except that lithium manganese iron phosphate is replaced by lithium iron phosphate.

[0123] Embodiment 4:

[0124] In this embodiment, a composite positive electrode material was prepared by the following method. The parameters of each component in the preparation are shown in Table 2 and Table 4.

[0125] Experimental method: basically the same as Example 1, except that the conductive functional material is Ketjen black coated polystyrene.

[0126] Embodiment 5:

[0127] In this embodiment, a composite positive electrode material was prepared by the following method. The parameters of each component in the preparation are shown in Table 2 and Table 4.

[0128] Experimental method: basically the same as Example 1, except that the conductive functional material is acetylene black coated polyurethane.

[0129] Embodiment 5:

[0130] In this embodiment, a composite positive electrode material was prepared by the following method. The parameters of each component in the preparation are shown in Table 2 and Table 4.

[0131] Experimental method: basically the same as Example 1, except that the conductive functional material is acetylene black coated polyurethane.

[0132] Embodiment 6:

[0133] In this embodiment, a composite positive electrode material was prepared by the following method. The parameters of each component in the preparation are shown in Table 2 and Table 4.

[0134] Experimental method: basically the same as Example 1, except that the insulating material is titanium dioxide.

[0135] Embodiment 7:

[0136] In this embodiment, a composite positive electrode material was prepared by the following method. The parameters of each component in the preparation are shown in Table 2 and Table 4.

[0137] Experimental method: basically the same as Example 1, except that the insulating material is magnesium oxide.

[0138] Embodiment 8:

[0139] In this embodiment, a composite positive electrode material was prepared by the following method. The parameters of each component in the preparation are shown in Table 2 and Table 4.

[0140] Experimental method: basically the same as Example 1, except that the particle size D 50(1) The particle size D is 15 μm. 50(2) The ternary material (NCM811) is 2μm, and the diameter D 3 The conductive functional material (graphene coated polyethylene) is 3 μm in diameter. 4 The 20nm aluminum oxide is fused at high speed to form a composite positive electrode material. 1 The second hole D is 6 μm. 2 It is 80nm.

[0141] Embodiment 9:

[0142] In this embodiment, a composite positive electrode material was prepared by the following method. The parameters of each component in the preparation are shown in Table 2 and Table 4.

[0143] Experimental method: basically the same as Example 1, except that the particle size D 50(1) The particle size D is 30 μm. 50(2) The ternary material (NCM811) is 5μm, and the diameter D 3 Conductive functional material (graphene coated polyethylene) with a diameter of 8 μm 4 100nm aluminum oxide is fused at high speed to form a composite positive electrode material.

[0144] Among them, the first hole D 1 The second hole D is 10 μm. 2 is 200nm.

[0145] Embodiment 10:

[0146] In this embodiment, a composite positive electrode material was prepared by the following method. The parameters of each component in the preparation are shown in Table 2 and Table 4.

[0147] Experimental method: basically the same as Example 1, except that the particle size D 50(1) The particle size D is 20 μm. 50(2) The diameter of the ternary material (NCM811) is 3 μm, the diameter of the second active material (lithium iron phosphate) is 5 μm, and the diameter D 3 The conductive functional material (graphene coated polyethylene) is 5 μm in diameter. 4 Alumina with a thickness of 50nm is fused mechanically at high speed to form a composite positive electrode material.

[0148] Among them, the first hole D 1 The second hole D is 8μm. 2 is 100nm.

[0149] Embodiment 11:

[0150] In this embodiment, a composite positive electrode material was prepared by the following method. The parameters of each component in the preparation are shown in Table 2 and Table 4.

[0151] Experimental method: basically the same as Example 1, except that the particle size D 50(1) The particle size D is 20 μm. 50(2) The ternary material (NCM811) with a diameter of 3 μm, the second active material (lithium manganate) with a diameter of 5 μm, and the diameter D 3 The conductive functional material (graphene coated polyethylene) is 5 μm in diameter. 4 Alumina with a thickness of 50nm is fused mechanically at high speed to form a composite positive electrode material.

[0152] Among them, the first hole D 1 The second hole D is 8μm. 2is 100nm.

[0153] Comparative Example 1:

[0154] In this comparative example, a positive electrode material was prepared by the following method, and the parameters of each component in the preparation are referred to Table 3 and Table 4.

[0155] Experimental method: The particle size D 50(1) The diameter of lithium manganese iron phosphate is 20 μm. 3 Conductive functional material (graphene coated polyethylene) with a diameter of 5 μm 4 Alumina with a thickness of 50nm is fused mechanically at high speed to form a composite positive electrode material.

[0156] Among them, the first hole D 1 8μm.

[0157] Comparative Example 2:

[0158] In this comparative example, a positive electrode material was prepared by the following method, and the parameters of each component in the preparation are referred to Table 3 and Table 4.

[0159] Experimental method: The particle size D 50(1) The particle size D is 20 μm. 50(2) The ternary material (NCM811) is 3μm, and the diameter D 4 Alumina with a thickness of 50nm is fused mechanically at high speed to form a composite positive electrode material.

[0160] Among them, the first hole D 1 The second hole D is 8μm. 2 is 100nm.

[0161] Comparative Example 3:

[0162] In this comparative example, a positive electrode material was prepared by the following method, and the parameters of each component in the preparation are referred to Table 3 and Table 4.

[0163] Experimental method: The particle size D 50(1) The particle size D is 20 μm. 50(2) The ternary material (NCM811) is 3μm, and the diameter D 3 It is a 5μm conductive functional material (graphene coated polyethylene).

[0164] Among them, the first hole D 1 The second hole D is 8μm. 2 is 100nm.

[0165] Comparative Example 4:

[0166] In this comparative example, a positive electrode material was prepared by the following method, and the parameters of each component in the preparation are referred to Table 3 and Table 4.

[0167] Experimental method: The particle size D 50(1) The particle size D of lithium manganese iron phosphate is 10 μm 50(2) The ternary material (NCM811) is 10 μm, and the diameter D 3 Conductive functional material (graphene coated polyethylene) with a diameter of 10 μm 4 Alumina with a thickness of 10 μm is fused mechanically at high speed to form a composite positive electrode material.

[0168] Comparative Example 5:

[0169] In this comparative example, a positive electrode material was prepared by the following method, and the parameters of each component in the preparation are referred to Table 3 and Table 4.

[0170] Experimental method: The particle size D 50(1) The particle size D of lithium manganese iron phosphate is 3 μm 50(2) The ternary material (NCM811) is 20 μm, and the diameter D 3 The conductive functional material (graphene coated polyethylene) is 5 μm in diameter. 4 Alumina with a thickness of 50nm is fused mechanically at high speed to form a composite positive electrode material.

[0171] Among them, the first hole D 1 is 100nm, the second hole D 2 8μm.

[0172] Comparative Example 6:

[0173] In this comparative example, a positive electrode material was prepared by the following method, and the parameters of each component in the preparation are referred to Table 3 and Table 4.

[0174] Experimental method: The particle size D 50(1) The particle size D is 20 μm. 50(2) The ternary material (NCM811) is 3μm, and the diameter D 3 The conductive functional material (graphene coated polyethylene) is 5 μm in diameter. 4 Alumina with a thickness of 5 μm is fused mechanically at high speed to form a composite positive electrode material.

[0175] Among them, the first hole D 1 The second hole D is 8μm. 2 is 100nm.

[0176] Comparative Example 7:

[0177] In this comparative example, a positive electrode material was prepared by the following method, and the parameters of each component in the preparation are referred to Table 3 and Table 4.

[0178] Experimental method: The particle size D50(1) The particle size D of lithium manganese iron phosphate is 3 μm 50(2) The ternary material (NCM811) is 20 μm, and the diameter D 3 The conductive functional material (graphene coated polyethylene) is 5 μm in diameter. 4 Alumina with a thickness of 5 μm is fused mechanically at high speed to form a composite positive electrode material.

[0179] Among them, the first hole D 1 is 100nm, the second hole D 2 8μm.

[0180] Comparative Example 8:

[0181] In this comparative example, a positive electrode material was prepared by the following method, and the parameters of each component in the preparation are referred to Table 3 and Table 4.

[0182] Experimental method: This comparative example is basically the same as Example 1, except that: in the preparation method of the composite positive electrode material, lithium manganese iron phosphate, ternary material (NCM811), conductive functional material (graphene-coated polyethylene) and aluminum oxide are not mixed and stirred at high speed.

[0183] Horizontal comparison test:

[0184] Test method:

[0185] (1) dispersing 96%, 1.5% and 2.5% by weight of a lithium-ion battery positive electrode material, a conductive agent and a binder in a solvent to obtain a positive electrode active slurry;

[0186] (2) The positive electrode active slurry is coated on aluminum foil and vacuum dried to obtain a positive electrode sheet; wherein the conductive agent is acetylene black, the binder is polyvinyl fluoride, and the solvent is N-methylpyrrolidone.

[0187] (3) The positive electrode sheet, separator and negative electrode sheet are stacked to obtain a battery cell, which is then placed into a casing and injected with electrolyte to assemble into a battery and tested on a blue battery test system; wherein the negative electrode sheet is a lithium sheet, the separator is Celgard3000, and the electrolyte is 0.25M lithium hexafluorophosphate.

[0188] Test 1: The method of powder compaction test is: after the positive electrode sheet is rolled by a roller press to a set compaction, it is folded in half manually, and the sheet is bent until the two folded sides are completely fitted together and then the crease is checked. The highest compaction that can keep the sheet crease opaque is the ultimate compaction of the sheet. The test results are shown in the table below.

[0189] Test 2: The positive electrode conductivity of the positive electrode sheet is tested. The test conditions are: the conductivity of the positive electrode material surface of the positive electrode sheet is tested using the Huace high temperature four-probe tester HEST800.

[0190] Test 3: The initial gram capacity is tested under the following conditions: fully charge the battery at room temperature (25°C), then discharge it at a rate of 1C to the cut-off voltage (2.5V) after it has been fully left at room temperature, and record the released capacity (energy).

[0191] Test 4: The batteries prepared in Examples 1-3 and Comparative Examples 1-16 were charged at a constant current of 1C at room temperature of 25°C, with a cut-off current of 0.05C, rested for 10 min, and discharged at 0.7C for 1000 cycles, and the capacity retention rate (%) after 1000 cycles was calculated.

[0192] Test 5: The needle puncture test is to prepare the single battery according to the regulations, and then use a Φ5mm~Φ8mm high-temperature resistant steel needle (the cone angle of the needle tip is 45°~60°, the surface of the needle is smooth, free of rust, oxide layer and oil) to penetrate the battery plate at a speed of (25±5)mm / s from a direction perpendicular to the battery plate. The penetration position should be close to the geometric center of the puncture surface, and the steel needle stays in the battery; observe for 1h.

[0193] Table 5. Performance test results of the batteries prepared in the examples and comparative examples in test 1 (unit: g / cm 3 )

[0194]

[0195] Table 6 Performance test results of batteries prepared in Examples and Comparative Examples in Test 2 (unit: S / cm)

[0196]

[0197] Table 7 Performance test results of batteries prepared in Examples and Comparative Examples in Test 3 (unit: mAh / g)

[0198]

[0199] Table 8 Performance test results of batteries prepared in Examples and Comparative Examples in Test 4 (unit: %)

[0200]

[0201] Table 9 Performance test results of batteries prepared in Examples and Comparative Examples in Test 5

[0202]

[0203] In the above table, the data format under the Acupuncture Test column is: number of qualified times / total number of times.

[0204] The following conclusions can be drawn from the performance test results in Tables 5 to 9:

[0205] (1) The composite positive electrode materials proposed in Examples 1-11 have excellent gram capacity, compaction density and cycle performance.

[0206] (2) Comparison between Comparative Example 1 and Example 1: The composite positive electrode material does not contain ternary materials, which will affect the initial gram capacity of the battery.

[0207] (3) Comparison between Example 2 and Example 1: The composite positive electrode material does not contain a conductive functional material, which makes it impossible to form a conductive network inside the material, which will affect the conductivity of the electrode sheet and thus affect the cycle performance of the battery.

[0208] (4) Comparison between Example 3 and Example 1: The composite positive electrode material does not contain insulating material. The insulating material has strong thermal stability and promotes the structural stability of the ternary material to a certain extent. The lack of insulating material will affect the cycle performance and safety performance of the battery.

[0209] (5) Comparison between Example 4 and Example 1: The particle sizes of lithium manganese iron phosphate, ternary material, conductive functional material and aluminum oxide are the same. After high-speed mechanical fusion, the core-shell structure proposed in the present invention is not formed, which will affect the compaction density and conductivity of the electrode, thereby affecting the gram capacity and cycle performance of the battery.

[0210] (6) Comparison of Example 5 and Example 1: Filling lithium manganese iron phosphate into the ternary material will increase the gram capacity of the material, but will affect the filling ratio of aluminum oxide and affect the safety performance of the battery.

[0211] (7) Comparison Example 6 with Example 1: Aluminum oxide is not filled in the ternary material. Since the thermal stability of the ternary material during use is worse than that of other positive electrode materials, such as lithium manganese iron phosphate, the heat dissipation effect of the positive electrode material will be weakened, and the diffusion rate of lithium ions cannot be adjusted, which will eventually affect the cycle performance and safety performance of the battery.

[0212] (8) Comparison of Example 7 and Example 1: When lithium manganese iron phosphate is filled into the ternary material, the gram capacity of the material will increase, but it will affect the safety performance of the battery. Aluminum oxide is not filled into the ternary material, and the battery cannot pass the needle puncture test 100%.

[0213] (9) Comparative Example 8: Compared with the embodiment, high-speed mixing was not performed, and the properties of the composite material formed were relatively poor.

[0214] The above are preferred implementation modes and corresponding embodiments of the present invention. It should be pointed out that, for those skilled in the art, without departing from the creative concept of the present invention, several modifications and improvements may be made, including but not limited to the adjustment of proportions, processes, dosages and reaction vessels, which all fall within the scope of protection of the present invention.

Claims

1. A composite positive electrode material, It is characterized in that include: A first active material, a ternary material, a conductive functional material and an insulating material; The first active material has a first hole on its surface; The surface of the ternary material is provided with a second hole; The conductive functional material and the ternary material can both be placed in the first hole; The insulating material can be placed in the second hole; The conductive functional material is a core-shell composite structure with a conductive material as the core and a thermosensitive polymer as the shell.

2. The composite positive electrode material according to claim 1, It is characterized in that The first active material, the ternary material, the conductive functional material and the insulating material meet the following relationship: D 50(1) >D 1 >D 3 ≥D 50(2) >D 2 >D 4 ; Among them, D 1 represents the diameter of the first hole; D 2 represents the diameter of the second hole; D 3 represents the diameter of the conductive functional material; D 4 Represents the diameter of the insulating material; D 50(1) D represents the first active material 50 ;D 50(2) D represents the ternary material 50 .

3. The composite positive electrode material according to claim 2, It is characterized in that The D of the first active material 50(1) The range is 10-50μm; The D of the ternary material 50(2) The range is 0.1-5μm; D 1 The range is 1-10μm; D 2 The range is 50-200nm; D 3 The range is 1-10μm; D 4 The range is 10-100nm.

4. The composite positive electrode material according to claim 1, It is characterized in that The insulating material includes at least one of aluminum oxide, boehmite, silicon dioxide, zirconium dioxide, titanium dioxide, magnesium oxide, zinc oxide, and calcium oxide.

5. The composite positive electrode material according to claim 1, It is characterized in that The thermosensitive polymer includes at least one of polyethylene, polypropylene, polyamide, polyesteramide, polystyrene, polyvinyl chloride, polyester, polyurethane, ethylene vinyl acetate polymer, ethylene acrylate polymer, olefin copolymer, propylene copolymer and ethylene copolymer.

6. The composite positive electrode material according to claim 1, It is characterized in that The conductive material includes at least one of polypyrrole, polythiophene, Ketjen black, conductive fiber, acetylene black, carbon nanotube, graphene, flake graphite, silicon carbide, molybdenum disilicide and lanthanum cobaltate.

7. The composite positive electrode material according to claim 1, It is characterized in that The composite positive electrode material also includes a second active material; The second active material includes at least one of an olivine-structured lithium manganese iron phosphate material, a layered polyacid lithium, a spinel-type lithium manganate, a layered manganese-rich lithium base, an olivine-type lithium iron phosphate, and an olivine-type lithium manganese phosphate.

8. The composite positive electrode material according to claim 1, It is characterized in that The first active material includes at least one of an olivine-structured lithium manganese iron phosphate material, a layered polyacid lithium, a spinel-type lithium manganate, a layered manganese-rich lithium base, an olivine-type lithium iron phosphate, and an olivine-type lithium manganese phosphate.

9. A method for preparing the composite positive electrode material according to any one of claims 1 to 8, It is characterized in that include: The first active material, the ternary material, the conductive functional material and the insulating material are fused by high-speed mechanical fusion, so that the conductive functional material enters the first holes on the surface of the first active material, and the insulating material enters the second holes on the surface of the ternary material, to obtain the composite positive electrode material.

10. The method for preparing the composite positive electrode material according to claim 9, It is characterized in that The step of fusing the first active material, the ternary material, the conductive functional material and the insulating material by a high-speed mechanical fusion method further includes: A second active material is added so that the second active material and the conductive functional material enter the first pores on the surface of the first active material through the high-speed mechanical fusion method.

11. A positive electrode sheet, It is characterized in that Comprising the composite positive electrode material as described in any one of claims 1 to 8.

12. A battery, It is characterized in that Comprising the positive electrode sheet as claimed in claim 11.

13. An electrical device, It is characterized in that A battery as claimed in claim 12 is used.

Citation Information

Patent Citations

  • Rate type nickel-cobalt-manganese positive electrode material and preparation method and application thereof

    CN111682192A

  • High-nickel positive electrode material, preparation method thereof and secondary battery