A high-capacity lithium battery positive electrode sheet and preparation method thereof

By using a combination of conductive graphene, conductive carbon nanotubes and modified polymers in the lithium battery cathode sheet, an efficient conductive and bonding network is formed, which solves the problem of low capacity retention of the lithium battery cathode sheet after cycling and improves efficiency. Capacitance and Cycling Stability.

CN118472261BActive Publication Date: 2024-10-29NANJING HANRUI NEW MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410764646.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-29
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

Existing lithium battery cathode sheets have a low capacity retention rate after cyclic charge and discharge, mainly due to high internal resistance and reduced adhesion, resulting in reduced electrical performance.

Method used

Using a specific proportion of conductive agent and binder combination, including conductive graphene, conductive carbon nanotubes, boric acid-modified polyvinyl alcohol and dopamine-modified polyacrylic acid, the compaction density is increased by forming a three-dimensional conductive network and a modified bonding network and cycle stability, reducing battery internal resistance.

Benefits of technology

It effectively improves the capacitance and cycle performance of the lithium battery cathode sheet, maintains high capacity, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of lithium battery positive electrode, specifically a high-capacity lithium battery positive electrode sheet and a preparation method thereof. The high-capacity lithium battery positive electrode sheet comprises a metal foil and a positive electrode slurry layer on its surface; the raw materials of the positive electrode slurry layer comprise the following substances: by weight, 85-90 parts of positive electrode active material, 1-2 parts of lithium carbonate, 4-6 parts of conductive agent, 5-7 parts of binder, 0.005-0.01 parts of initiator, and 50-60 parts of solvent. The positive electrode active material comprises one or more of lithium iron phosphate, lithium manganese iron phosphate, lithium manganate, lithium cobaltate, lithium nickelate, and lithium nickel cobalt manganate. The conductive agent comprises conductive graphene and conductive carbon nanotubes in a mass ratio of 1:3. The binder comprises boric acid-modified polyvinyl alcohol and dopamine-modified polyacrylic acid in a mass ratio of 3.8-4:1-1.2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium battery positive electrodes, and in particular to a high-capacity lithium battery positive electrode sheet and a preparation method thereof. Background Art

[0002] The rapid development of the new energy market has accelerated the development of lithium-ion batteries; the preparation of lithium batteries with high specific capacity, good cycle stability and environmental friendliness has also received widespread attention. Among them, the positive electrode, one of the important components of lithium batteries, has a direct impact on battery capacity and cycle performance; with the in-depth study of lithium-ion battery related technologies, it is found that the key to affecting the practical application value lies in the service life, and the key to the service life lies in reducing the irreversible capacity decay during the cycle; in the prior art, although the prepared lithium battery positive electrode has a high capacity at the beginning, after cyclic charge and discharge, the high capacity decreases significantly and the retention rate is low; therefore, it is necessary to further improve this shortcoming so that it can still maintain a high capacity after the cycle.

[0003] Lithium battery positive plates are generally made by combining positive electrode slurry containing electrode active materials, conductive agents, and binders on the surface of a metal foil layer. Among them, the reasons that affect the high capacity retention rate of lithium battery positive plates include the following aspects: First, after the positive electrode slurry forms a coating, the internal resistance is high and the lithium ion diffusion coefficient is low, resulting in poor electrical performance; second, during the cyclic charge and discharge process, the adhesion is reduced due to stress, resulting in the shedding of active materials, and the impedance between the metal foil and the positive electrode slurry layer increases, resulting in a significant decline in performance.

[0004] In summary, solving the above problems and preparing a high-capacity lithium battery positive electrode sheet with high capacity retention rate after cycling has important application value. Summary of the invention

[0005] The object of the present invention is to provide a high-capacity lithium battery positive electrode sheet and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A high-capacity lithium battery positive electrode sheet, the high-capacity lithium battery positive electrode sheet comprising a metal foil and a positive electrode slurry layer on its surface; the raw materials of the positive electrode slurry layer comprise the following substances: by weight, 85 to 90 parts of positive electrode active material, 1 to 2 parts of lithium carbonate, 4 to 6 parts of conductive agent, 5 to 7 parts of binder, 0.005 to 0.01 parts of initiator, and 50 to 60 parts of solvent.

[0008] In a further embodiment, the positive electrode active material includes one or more of lithium iron phosphate, lithium manganese iron phosphate, lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, and lithium nickel cobalt manganese oxide.

[0009] In a further embodiment, the conductive agent includes conductive graphene and conductive carbon nanotubes in a mass ratio of 1:3.

[0010] In a further embodiment, the binder includes boric acid-modified polyvinyl alcohol and dopamine-modified polyacrylic acid in a mass ratio of 3.8-4:1-1.2.

[0011] In a further embodiment, the preparation method of the boric acid-modified polyvinyl alcohol is:

[0012] (1) Add polyvinyl alcohol to deionized water, stir and dissolve at 90-95°C; cool to 60-65°C, add 4-dimethylaminopyridine, and stir evenly; add maleic anhydride, stir and react for 12-24 hours; wash and freeze-dry to obtain maleic anhydride-modified polyvinyl alcohol;

[0013] (2) Add maleic anhydride-modified polyvinyl alcohol, mercaptophenylboric acid, and a photoinitiator to deionized water in sequence, stir, and irradiate for reaction under 295-395 nm ultraviolet light at 5-10 mW / cm2 for 2-5 minutes; wash and freeze-dry to obtain boric acid-modified polyvinyl alcohol.

[0014] In a further embodiment, in the raw material of maleic anhydride-modified polyvinyl alcohol, the mass ratio of polyvinyl alcohol to maleic anhydride is 1:4-5; in the raw material of boric acid-modified polyvinyl alcohol, the mass ratio of maleic anhydride-modified polyvinyl alcohol to mercaptophenylboric acid is 10:0.6-0.8.

[0015] In a further scheme, the preparation method of the dopamine-modified polyacrylic acid is: add polyacrylic acid to deionized water, add 1-ethyl-3-(3-dimethylaminopropyl) carbodiimide, dopamine, and 4-aminomethyl-piperidine-1-carboxylic acid allyl ester, adjust the pH to 5.5±0.2, and stir the reaction at room temperature for 12 to 16 hours; wash and freeze-dry to obtain dopamine-modified polyacrylic acid.

[0016] In a further embodiment, the mass ratio of the polyacrylic acid, dopamine, and 4-aminomethyl-piperidine-1-carboxylic acid allyl ester is 10:1.5~2.2:0.3~0.5.

[0017] In a further embodiment, a method for preparing a high-capacity lithium battery positive electrode sheet comprises the following steps:

[0018] Step 1: Under light-proof conditions, add a conductive agent to deionized water, add 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide, and stir for 0.5 to 1 hour; add cysteine, stir at 40 to 50° C. for 4 to 5 hours, stir at room temperature for 12 to 24 hours, wash, and freeze-dry to obtain raw material A;

[0019] Step 2: Under light-proof conditions, add the positive electrode active material, lithium carbonate, raw material A, initiator, and binder to the solvent in sequence, and homogenize to obtain a positive electrode slurry;

[0020] Step 3: Coat the positive electrode slurry on the surface of the metal foil, expose it to ultraviolet light, dry it at 60-80°C, and compact it to obtain a positive electrode slurry layer to obtain a high-capacity lithium battery positive electrode sheet.

[0021] Compared with the prior art, the present application has the following beneficial effects: in the scheme, a conductive agent of a specific proportion and a binder of a specific component are introduced into the positive electrode slurry, thereby effectively improving the compaction density, reducing the internal resistance of the battery, and thus increasing the capacity; at the same time, by modifying the components in the binder, the bonding force during the charge and discharge process is effectively suppressed, thereby increasing the electrical cycle performance of the positive electrode sheet of the lithium battery.

[0022] (1) The conductive agent is composed of conductive graphene and conductive carbon nanotubes. Compared with the common single conductive agent, the mixed conductive agent can form a three-dimensional conductive network of points, lines and surfaces, thereby improving the ion transmission performance and effectively increasing the battery capacity. On the other hand, the scheme defines a specific ratio. When the composite ratio is 1:3, it has a more optimized compaction density and the smallest internal resistance of the battery, thereby improving the increase in internal resistance after cycling and improving the cycle electrical performance of the lithium battery positive electrode, thereby ensuring a high capacity retention rate.

[0023] (2) The binder is a composite of boric acid-modified polyvinyl alcohol and dopamine-modified polyacrylic acid. Compared with a single conductive agent, the two binders can synergistically improve the cycle performance of the positive electrode of a lithium battery.

[0024] Among them, polyvinyl alcohol is a semi-crystalline polymer containing hydroxyl groups with good charge discharge capacity. It has high adhesion to metal foil. At the same time, its high crystallinity and good thermal stability are beneficial to maintain the interface stability between the positive electrode slurry and the metal foil when the volume expands during the cyclic charge and discharge process, thereby improving the retention rate of high capacity after the cycle. However, due to high crystallinity, there is migration resistance of electrons and ions in the electrode, and residual stress exists during the drying and curing process, which makes the internal resistance greater. Therefore, polyvinyl alcohol is further modified by first using maleic anhydride to graft carboxyl groups on its surface, and then using the double bonds in maleic anhydride to graft mercaptophenylboric acid; grafting carboxyl groups and boric acid groups on its chain segments is beneficial to improve adhesion and electrical properties. However, it should be noted that after modification, the degree of crystallinity decreases, which will reduce the cyclability, but the introduction of boron groups makes up for the defects to a certain extent.

[0025] On the other hand, dopamine-modified polyacrylic acid is further introduced to form strong hydrogen bonds between dopamine and boric acid, further strengthening the stability of the bonding network during the cycle. The introduction of dopamine-modified polyacrylic acid further increases the compaction density, and polyacrylic acid contains a large number of carboxyl groups, which improves the electrical properties and cycle performance; however, compared with polyvinyl alcohol, its ability to protect the surface of active substances from electrolyte degradation is weaker, so its introduction is only for reinforcement, and the amount added should not be too much. Too much is not conducive to electrical cycle performance. The optimal ratio is: the optimal ratio of boric acid-modified polyvinyl alcohol and dopamine-modified polyacrylic acid is 3.8~4:1~1.2.

[0026] In addition, in the scheme, during the preparation and coating process of the positive electrode slurry, the conductive agent is further modified with cysteine ​​to improve the dispersibility of the conductive agent while allowing the surface of the conductive agent to contain thiol groups, which can cross-link with boric acid-modified polyvinyl alcohol and dopamine-modified polyacrylic acid to play the role of a connector, thereby improving the cycle stability and adhesion of the bonding network; at the same time, since the positive electrode slurry is UV-crosslinked before drying and curing, the stress during drying and curing is suppressed, the thermal curing mobility of the substances in the positive electrode slurry layer during the curing process is reduced, and the dispersibility of the positive electrode slurry layer is improved, thereby improving the battery performance and cycle stability. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] It should be noted that there are no special restrictions on the purchase manufacturers of all raw materials involved in the present invention, and exemplarily include: In the following embodiments, the parts are by mass, among the raw materials: the product number of the conductive carbon nanotube is 180111144602, which is a short carboxylated multi-walled carbon nanotube powder conductive carbon nanotube, and the brand is Cramar; the product number of the conductive graphene is 180116160435, which is a conductive carboxylated graphene, and the brand is Cramar; the CAS number of 4-aminomethyl-piperidine-1-carboxylic acid allyl ester is 885274-93-1; the degree of hydrolysis of polyvinyl alcohol is 98%, and the molecular weight is about 16000; the molecular weight of polyacrylic acid is about 5000; all are commercially purchased.

[0029] Embodiment 1: A method for preparing a high-capacity lithium battery positive electrode sheet, comprising the following steps:

[0030] Pre-preparation: (1) Add 1 part of polyvinyl alcohol to 10 parts of deionized water, stir and dissolve at 95°C; cool to 65°C, add 0.3 parts of 4-dimethylaminopyridine, and stir evenly; add 4.5 parts of maleic anhydride, stir and react for 4 hours; wash and freeze-dry to obtain maleic anhydride-modified polyvinyl alcohol; add 10 parts of maleic anhydride-modified polyvinyl alcohol, 0.72 parts of 4-mercaptophenylboric acid, and 0.5 parts of photoinitiator I2959 to deionized water in sequence, stir, and irradiate under 365nm ultraviolet light at 10mW / cm 2 , react under light for 5 minutes; wash and freeze-dry to obtain boric acid-modified polyvinyl alcohol.

[0031] (2) Add 10 parts of polyacrylic acid to 100 parts of deionized water, add 1.5 parts of 1-ethyl-3-(3-dimethylaminopropyl) carbodiimide, 2 parts of dopamine, and 0.5 parts of 4-aminomethyl-piperidine-1-carboxylic acid allyl ester, adjust the pH to 5.5, and stir the reaction at room temperature for 12 hours; wash and freeze-dry to obtain dopamine-modified polyacrylic acid.

[0032] Step 1: (1) Mix conductive graphene and conductive carbon nanotubes in a mass ratio of 1:3 to obtain a conductive agent; add 5 parts of the conductive agent to deionized water under light protection, add 1 part of 1-ethyl-3-(3-dimethylaminopropyl) carbodiimide, and stir for 1 hour; add 0.8 parts of cysteine, stir at 50°C for 5 hours, stir at room temperature for 24 hours, wash, and freeze-dry to obtain raw material A;

[0033] (2) Evenly mixing boric acid-modified polyvinyl alcohol and dopamine-modified polyacrylic acid in a mass ratio of 4:1 to obtain a binder;

[0034] Step 2: Under light protection, 89 parts of lithium nickel cobalt manganese oxide NCM622, 1 part of lithium carbonate, raw material A, 0.005 parts of photoinitiator AIBN, and 5 parts of binder are sequentially added to 50 parts of N-methylpyrrolidone, and homogenized to obtain a positive electrode slurry;

[0035] Step 3: Coat the positive electrode slurry on the surface of the metal foil and expose it to 365nm ultraviolet light at 10mW / cm 2 , irradiated with ultraviolet light for 10 minutes, dried at 80°C, compacted to obtain a positive electrode slurry layer, and thus a high-capacity lithium battery positive electrode sheet was obtained.

[0036] Embodiment 2: A method for preparing a high-capacity lithium battery positive electrode sheet, comprising the following steps:

[0037] Pre-preparation: (1) Add 1 part of polyvinyl alcohol to 10 parts of deionized water, stir and dissolve at 95°C; cool to 65°C, add 0.3 parts of 4-dimethylaminopyridine, and stir evenly; add 4.5 parts of maleic anhydride, stir and react for 4 hours; wash and freeze-dry to obtain maleic anhydride-modified polyvinyl alcohol; add 10 parts of maleic anhydride-modified polyvinyl alcohol, 0.72 parts of 4-mercaptophenylboric acid, and 0.5 parts of photoinitiator I2959 to deionized water in sequence, stir, and irradiate under 365nm ultraviolet light at 10mW / cm 2 , react under light for 5 minutes; wash and freeze-dry to obtain boric acid-modified polyvinyl alcohol.

[0038] (2) Add 10 parts of polyacrylic acid to 100 parts of deionized water, add 1.5 parts of 1-ethyl-3-(3-dimethylaminopropyl) carbodiimide, 2 parts of dopamine, and 0.5 parts of 4-aminomethyl-piperidine-1-carboxylic acid allyl ester, adjust the pH to 5.5, and stir the reaction at room temperature for 12 hours; wash and freeze-dry to obtain dopamine-modified polyacrylic acid.

[0039] Step 1: (1) Mix conductive graphene and conductive carbon nanotubes in a mass ratio of 1:3 to obtain a conductive agent; add 4 parts of the conductive agent to deionized water under light protection, add 1 part of 1-ethyl-3-(3-dimethylaminopropyl) carbodiimide, and stir for 1 hour; add 0.8 parts of cysteine, stir at 50°C for 5 hours, stir at room temperature for 24 hours, wash, and freeze-dry to obtain raw material A;

[0040] (2) Evenly mixing boric acid-modified polyvinyl alcohol and dopamine-modified polyacrylic acid in a mass ratio of 3.8:1.2 to obtain a binder;

[0041] Step 2: Under light protection, 87 parts of lithium nickel cobalt manganese oxide NCM622, 2 parts of lithium carbonate, raw material A, 0.005 parts of photoinitiator AIBN, and 7 parts of binder are sequentially added to 50 parts of N-methylpyrrolidone, and homogenized to obtain a positive electrode slurry;

[0042] Step 3: Coat the positive electrode slurry on the surface of the metal foil and expose it to 365nm ultraviolet light at 10mW / cm 2 , irradiated with ultraviolet light for 10 minutes, dried at 80°C, compacted to obtain a positive electrode slurry layer, and thus a high-capacity lithium battery positive electrode sheet was obtained.

[0043] Embodiment 3: A method for preparing a high-capacity lithium battery positive electrode sheet, comprising the following steps:

[0044] Pre-preparation: (1) Add 1 part of polyvinyl alcohol to 10 parts of deionized water, stir and dissolve at 95°C; cool to 65°C, add 0.3 parts of 4-dimethylaminopyridine, and stir evenly; add 4.5 parts of maleic anhydride, stir and react for 4 hours; wash and freeze-dry to obtain maleic anhydride-modified polyvinyl alcohol; add 10 parts of maleic anhydride-modified polyvinyl alcohol, 0.72 parts of 4-mercaptophenylboric acid, and 0.5 parts of photoinitiator I2959 to deionized water in sequence, stir, and irradiate under 365nm ultraviolet light at 10mW / cm 2 , react under light for 5 minutes; wash and freeze-dry to obtain boric acid-modified polyvinyl alcohol.

[0045] (2) Add 10 parts of polyacrylic acid to 100 parts of deionized water, add 1.5 parts of 1-ethyl-3-(3-dimethylaminopropyl) carbodiimide, 2 parts of dopamine, and 0.5 parts of 4-aminomethyl-piperidine-1-carboxylic acid allyl ester, adjust the pH to 5.5, and stir the reaction at room temperature for 12 hours; wash and freeze-dry to obtain dopamine-modified polyacrylic acid.

[0046] Step 1: (1) Mix conductive graphene and conductive carbon nanotubes in a mass ratio of 1:3 to obtain a conductive agent; add 4 parts of the conductive agent to deionized water under light protection, add 1 part of 1-ethyl-3-(3-dimethylaminopropyl) carbodiimide, and stir for 1 hour; add 0.8 parts of cysteine, stir at 50°C for 5 hours, stir at room temperature for 24 hours, wash, and freeze-dry to obtain raw material A;

[0047] (2) Evenly mixing boric acid-modified polyvinyl alcohol and dopamine-modified polyacrylic acid in a mass ratio of 4:1 to obtain a binder;

[0048] Step 2: Under light protection, 90 parts of lithium nickel cobalt manganese oxide NCM622, 1 part of lithium carbonate, raw material A, 0.005 parts of photoinitiator AIBN, and 5 parts of binder are sequentially added to 50 parts of N-methylpyrrolidone, and homogenized to obtain a positive electrode slurry;

[0049] Step 3: Coat the positive electrode slurry on the surface of the metal foil and expose it to 365nm ultraviolet light at 10mW / cm 2 , irradiated with ultraviolet light for 10 minutes, dried at 80°C, compacted to obtain a positive electrode slurry layer, and thus a high-capacity lithium battery positive electrode sheet was obtained.

[0050] Comparative Example 1: PVDF binder is used instead of the binder in Example 1, and the rest is the same as Example 1; the details are as follows:

[0051] Step 1: (1) Mix conductive graphene and conductive carbon nanotubes in a mass ratio of 1:3 to obtain a conductive agent; add 5 parts of the conductive agent to deionized water under light protection, add 1 part of 1-ethyl-3-(3-dimethylaminopropyl) carbodiimide, and stir for 1 hour; add 0.8 parts of cysteine, stir at 50°C for 5 hours, stir at room temperature for 24 hours, wash, and freeze-dry to obtain raw material A;

[0052] (2) Evenly mixing boric acid-modified polyvinyl alcohol and dopamine-modified polyacrylic acid in a mass ratio of 4:1 to obtain a binder;

[0053] Step 2: Under light protection, 89 parts of lithium nickel cobalt manganese oxide NCM622, 1 part of lithium carbonate, raw material A, 0.005 parts of photoinitiator AIBN, and 5 parts of PVDF binder are sequentially added to 50 parts of N-methylpyrrolidone, and homogenized to obtain a positive electrode slurry;

[0054] Step 3: Coat the positive electrode slurry on the surface of the metal foil and expose it to 365nm ultraviolet light at 10mW / cm 2 , irradiated with ultraviolet light for 10 minutes, dried at 80°C, compacted to obtain a positive electrode slurry layer, and thus a high-capacity lithium battery positive electrode sheet was obtained.

[0055] Comparative Example 2: Boric acid-modified polyvinyl alcohol is used alone as a binder, and the rest is the same as Example 1; the details are as follows:

[0056] Step 1: Evenly mix conductive graphene and conductive carbon nanotubes in a mass ratio of 1:3 to obtain a conductive agent; add 5 parts of the conductive agent to deionized water under light protection, add 1 part of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide, and stir for 1 hour; add 0.8 parts of cysteine, stir at 50°C for 5 hours, stir at room temperature for 24 hours, wash, and freeze-dry to obtain raw material A;

[0057] Step 2: Under light protection, 89 parts of lithium nickel cobalt manganese oxide NCM622, 1 part of lithium carbonate, raw material A, 0.005 parts of photoinitiator AIBN, and 5 parts of boric acid-modified polyvinyl alcohol were sequentially added to 50 parts of N-methylpyrrolidone, and homogenized to obtain a positive electrode slurry;

[0058] Step 3: Coat the positive electrode slurry on the surface of the metal foil and expose it to 365nm ultraviolet light at 10mW / cm 2 , irradiated with ultraviolet light for 10 minutes, dried at 80°C, compacted to obtain a positive electrode slurry layer, and thus a high-capacity lithium battery positive electrode sheet was obtained.

[0059] Comparative Example 3: Boric acid-modified polyvinyl alcohol and dopamine-modified polyacrylic acid in a mass ratio of 1:1 were used as binders, and the rest was the same as Example 1; the details are as follows:

[0060] Step 1: (1) Mix conductive graphene and conductive carbon nanotubes in a mass ratio of 1:3 to obtain a conductive agent; add 5 parts of the conductive agent to deionized water under light protection, add 1 part of 1-ethyl-3-(3-dimethylaminopropyl) carbodiimide, and stir for 1 hour; add 0.8 parts of cysteine, stir at 50°C for 5 hours, stir at room temperature for 24 hours, wash, and freeze-dry to obtain raw material A;

[0061] (2) Evenly mixing boric acid-modified polyvinyl alcohol and dopamine-modified polyacrylic acid in a mass ratio of 1:1 to obtain a binder;

[0062] Step 2: Under light protection, 89 parts of lithium nickel cobalt manganese oxide NCM622, 1 part of lithium carbonate, raw material A, 0.005 parts of photoinitiator AIBN, and 5 parts of binder are sequentially added to 50 parts of N-methylpyrrolidone, and homogenized to obtain a positive electrode slurry;

[0063] Step 3: Coat the positive electrode slurry on the surface of the metal foil and expose it to 365nm ultraviolet light at 10mW / cm 2 , irradiated with ultraviolet light for 10 minutes, dried at 80°C, compacted to obtain a positive electrode slurry layer, and thus a high-capacity lithium battery positive electrode sheet was obtained.

[0064] Comparative Example 4: Conductive graphene and conductive carbon nanotubes in a mass ratio of 1:1 were used as the conductive agent, and the rest was the same as Example 1; the details are as follows:

[0065] Step 1: (1) Mix conductive graphene and conductive carbon nanotubes in a mass ratio of 1:1 to obtain a conductive agent; add 5 parts of the conductive agent to deionized water under light protection, add 1 part of 1-ethyl-3-(3-dimethylaminopropyl) carbodiimide, and stir for 1 hour; add 0.8 parts of cysteine, stir at 50°C for 5 hours, stir at room temperature for 24 hours, wash, and freeze-dry to obtain raw material A;

[0066] (2) Evenly mixing boric acid-modified polyvinyl alcohol and dopamine-modified polyacrylic acid in a mass ratio of 4:1 to obtain a binder;

[0067] Step 2: Under light protection, 89 parts of lithium nickel cobalt manganese oxide NCM622, 1 part of lithium carbonate, raw material A, 0.005 parts of photoinitiator AIBN, and 5 parts of binder are sequentially added to 50 parts of N-methylpyrrolidone, and homogenized to obtain a positive electrode slurry;

[0068] Step 3: Coat the positive electrode slurry on the surface of the metal foil and expose it to 365nm ultraviolet light at 10mW / cm 2 , irradiated with ultraviolet light for 10 minutes, dried at 80°C, compacted to obtain a positive electrode slurry layer, and thus a high-capacity lithium battery positive electrode sheet was obtained.

[0069] Performance test: The positive electrode sheets prepared in the embodiment and the comparative example were loaded with 306 mg / cm 2 , conduct relevant point formation test, constant current mode, at 2.8~4.3V, first activate at 0.1C for 1 week, then test discharge capacity at 1C, and detect capacity retention after 200 cycles; the obtained data are shown in the following table:

[0070]

[0071] The data in the above table show that: in the scheme, a high-capacity lithium battery positive electrode sheet prepared effectively improves the compaction density, reduces the resistance, and the cycle adhesion through the specific components of the binder and the conductive agent; thereby effectively improving the capacity and cycle stability of the lithium battery positive electrode sheet. The data of comparative examples 1 to 4 show that: when PVDF is used as a binder, the internal resistance is large and the cycle stability is reduced, resulting in a decrease in performance; and the use of a single boric acid-modified polyvinyl alcohol, or the introduction of a high content of dopamine polyacrylic acid, leads to a decrease in electrical performance due to the influence on the stability of the binder, internal resistance and other related properties; in addition, the proportion of the conductive agent affects the overall compaction performance and internal resistance, thereby resulting in a decrease in electrical performance.

[0072] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A high-capacity lithium battery positive electrode, characterized in that: The high-capacity lithium battery positive electrode sheet comprises a metal foil and a positive electrode slurry layer on its surface; the raw materials of the positive electrode slurry layer comprise the following substances: by weight, 85 to 90 parts of positive electrode active material, 1 to 2 parts of lithium carbonate, 4 to 6 parts of conductive agent, 5 to 7 parts of binder, 0.005 to 0.01 parts of initiator, and 50 to 60 parts of solvent; The conductive agent is composed of conductive graphene and conductive carbon nanotubes in a mass ratio of 1:3; the conductive agent is pre-modified with cysteine; The binder is composed of boric acid-modified polyvinyl alcohol and dopamine-modified polyacrylic acid in a mass ratio of 3.8-4:1-1.

2.

2. The high-capacity lithium battery positive electrode according to claim 1, characterized in that: The positive electrode active material includes one or more of lithium iron phosphate, lithium manganese iron phosphate, lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, and lithium nickel cobalt manganese oxide.

3. The high-capacity lithium battery positive electrode according to claim 1, characterized in that: The preparation method of the boric acid modified polyvinyl alcohol is: (1) Add polyvinyl alcohol to deionized water, stir and dissolve at 90-95° C.; cool to 60-65° C., add 4-dimethylaminopyridine, and stir evenly; add maleic anhydride, and stir to react for 12-24 hours; washing and freeze-drying to obtain maleic anhydride-modified polyvinyl alcohol; (2) maleic anhydride-modified polyvinyl alcohol, mercaptophenyl boric acid, and photoinitiator are sequentially added to deionized water, stirred, and exposed to ultraviolet light at 295 to 395 nm at 5 to 10 mW / cm 2 , light reaction for 2 to 5 minutes; The product was washed and freeze-dried to obtain boric acid-modified polyvinyl alcohol.

4. The high-capacity lithium battery positive electrode according to claim 3, characterized in that: In the raw material of maleic anhydride-modified polyvinyl alcohol, the mass ratio of polyvinyl alcohol to maleic anhydride is 1:4-5; in the raw material of boric acid-modified polyvinyl alcohol, the mass ratio of maleic anhydride-modified polyvinyl alcohol to mercaptophenylboric acid is 10:0.6-0.

8.

5. The high-capacity lithium battery positive electrode according to claim 1, characterized in that: The preparation method of the dopamine-modified polyacrylic acid comprises: adding polyacrylic acid to deionized water, adding 1-ethyl-3-(3-dimethylaminopropyl) carbodiimide, dopamine, and 4-aminomethyl-piperidine-1-carboxylic acid allyl ester, adjusting the pH to 5.5±0.2, stirring and reacting at room temperature for 12 to 16 hours; washing, and freeze-drying to obtain the dopamine-modified polyacrylic acid.

6. A high-capacity lithium battery positive electrode according to claim 5, characterized in that: The mass ratio of the polyacrylic acid, dopamine and 4-aminomethyl-piperidine-1-carboxylic acid allyl ester is 10:1.5-2.2:0.3-0.

5.

7. A method for preparing a high-capacity lithium battery positive electrode sheet according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1: Under light-proof conditions, add a conductive agent to deionized water, add 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide, and stir for 0.5 to 1 hour; add cysteine, stir at 40 to 50° C. for 4 to 5 hours, stir at room temperature for 12 to 24 hours, wash, and freeze-dry to obtain raw material A; Step 2: Under light-proof conditions, add the positive electrode active material, lithium carbonate, raw material A, initiator, and binder to the solvent in sequence, and homogenize to obtain a positive electrode slurry; Step 3: Coat the positive electrode slurry on the surface of the metal foil, irradiate with ultraviolet light, dry at 60-80°C, and compact to obtain a positive electrode slurry layer to obtain a high-capacity lithium battery positive electrode sheet.

Citation Information

Patent Citations

  • High-safety lithium ion battery cathode paste and preparation method thereof

    CN105514417A

  • Tetrafluoro-borate ion crosslinking hydroxyl polymer binding agent, preparation method thereof, secondary battery and negative electrode and negative paste of secondary battery