A calcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker, cement composition and preparation method thereof

By calcining the monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker system under low temperature conditions and adding Li2O source, the problem of carbon dioxide emissions and high energy consumption caused by high-temperature calcination in cement production is solved. The production cost is reduced, the consolidation phenomenon is avoided, and the grinding efficiency is improved.

CN118479760BActive Publication Date: 2024-10-15UNIV OF JINAN
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410938798.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-15
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

High-temperature calcination during the cement production process results in large amounts of carbon dioxide emissions and high energy consumption, and the production cost of sulfoaluminate cement is high, making it difficult to replace ordinary Portland cement.

Method used

Using monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker system, calcium sulfosilicate is burned under low temperature conditions below 1200°C, and Li2O source is added as a catalyst in the preparation to destroy disilicate. The structural stability of tricalcium reduces the calcination temperature and calcium content and avoids consolidation.

Benefits of technology

It significantly reduces the calcination temperature and energy consumption of cement clinker, reduces carbon dioxide emissions, solves the consolidation problem caused by tricalcium disilicate, and improves grinding efficiency and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118479760B_ABST
    Figure CN118479760B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of cement clinker preparation, and specifically discloses a calcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker, a cement composition and a preparation method thereof. The cement clinker comprises: 6-12wt.% of calcium silicate, 27-45wt.% of calcium sulfosilicate, 36-55wt.% of dicalcium silicate, 0.48-3wt.% of calcite, and 1-4wt.% of glass phase. The method comprises: (1) taking 65-80 parts by weight of calcium raw materials, 43-65 parts by weight of siliceous raw materials, 22-38 parts by weight of gypsum, 0.5-2 parts by weight of Li2O source, and 0.1-1 parts by weight of calcium fluoride. (2) calcining the powder raw materials formed by the above raw materials at a temperature not higher than 1200°C, and after completion, quenching treatment is performed, and then grinding is performed to obtain the cement clinker. Not only the carbon emissions and energy consumption generated by the preparation of cement clinker are reduced, but also the problem that tricalcium disilicate is difficult to eliminate in the coexistence system of calcium silicate and dicalcium silicate is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cement clinker preparation, and in particular to a monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker, a cement composition and a preparation method thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] The world is increasingly concerned about climate change, and countries are actively taking measures to reduce greenhouse gas emissions. A large amount of carbon dioxide emissions will be generated during cement production, so the building materials industry has been included in the key targets of emission reduction. In response, the building materials industry has taken a variety of measures and methods to reduce carbon emissions during the production process, such as using alternative raw materials and recycled materials, actively promoting green building materials and high-performance building materials, researching and applying carbon capture and storage technologies, improving energy efficiency and resource utilization, and vigorously developing low-carbon cement clinker, etc., to promote the sustainable development of the cement industry.

[0004] For ordinary Portland cement, it takes about 1.3 tons of limestone to produce 1 ton of cement clinker, and the calcination temperature is as high as about 1450℃. The excessively high calcination temperature not only consumes a lot of fuel, but also releases a lot of carbon dioxide due to the decomposition of limestone and the combustion of fuel in the process. The calcination temperature of sulphoaluminate cement is about 1350℃, which is lower than that of ordinary Portland cement. Although it is beneficial to reduce carbon dioxide emissions, the firing of sulphoaluminate cement requires high-grade raw materials such as bauxite, resulting in excessively high production costs, making it difficult to replace ordinary Portland cement for large-scale use. Summary of the invention

[0005] The present invention provides a monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker, a cement composition and a preparation method thereof, which not only helps to reduce carbon emissions and energy consumption generated by cement clinker preparation, but also solves the problem that tricalcium disilicate is difficult to eliminate in a system where monocalcium silicate and dicalcium silicate coexist. Specifically, the technical solution of the present invention is as follows.

[0006] Firstly, the present invention discloses a monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker, comprising: 6-12wt.% of monocalcium silicate, 27-45wt.% of calcium sulfosilicate, 36-55wt.% of dicalcium silicate, 0.48-3wt.% of grossamite, 1-4wt.% of glass phase, and the remainder being unreacted raw materials and inevitable impurities.

[0007] Secondly, the present invention discloses a monocalcium silicate-calcium sulphosilicate-dicalcium silicate cement composition, comprising: 92-98 parts by weight of the monocalcium silicate-calcium sulphosilicate-dicalcium silicate cement clinker and 3-5 parts by weight of gypsum.

[0008] Again, the present invention discloses a method for preparing the monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker, comprising the following steps:

[0009] (1) Take the following raw materials: 65-80 parts by weight of calcium raw material, 43-65 parts by weight of silicon raw material, 22-38 parts by weight of gypsum, 2 0.5-2 parts by weight of O source, 0.1-1 parts by weight of calcium fluoride.

[0010] (2) The powdered raw material formed by the above raw materials is calcined at a temperature not higher than 1200° C., and then rapidly cooled and ground to obtain the cement clinker.

[0011] Furthermore, in step (1), the Li 2 The O source includes at least one of lithium slag, carbonate clay-type lithium ore, volcanic clay-type lithium ore, etc. Optionally, the Li 2 Li in O source 2 The mass fraction of O is not less than 0.5% in order to maintain effective catalysis.

[0012] Furthermore, in step (1), the calcium raw material includes but is not limited to at least one of limestone, carbide slag, quicklime, high-calcium fly ash, etc.

[0013] Furthermore, in step (1), the siliceous raw material includes but is not limited to at least one of sandstone, stripping soil, silica ash, coal gangue, etc.

[0014] Furthermore, in step (1), the gypsum includes but is not limited to: at least one of desulfurized gypsum, fluorinated gypsum, phosphogypsum, borogypsum, titanium gypsum, etc.

[0015] Furthermore, in step (2), the calcination temperature is 1075-1175° C., and the calcination time is 10-40 min.

[0016] Compared with the prior art, the technical solution of the present invention has at least the following beneficial effects:

[0017] Calcium sulfosilicate can be fired at low temperatures below 1200°C, which reduces the energy consumption required for preparing ordinary Portland cement, and requires less limestone. The formation temperatures of monocalcium silicate and dicalcium silicate are also below 1300°C, and the required calcium content is relatively low. Therefore, the cement clinker system formed by the calcium sulfosilicate, monocalcium silicate and dicalcium silicate of the present invention not only requires a low calcination temperature (not higher than 1200°C), but also significantly reduces the calcination temperature of 1450°C of traditional ordinary Portland cement and 1350°C of sulphoaluminate cement, which not only saves a lot of calcination heat consumption, but also requires less calcium raw materials (such as limestone, etc.), so that less carbon dioxide is released during calcination due to the decomposition of limestone.

[0018] However, the present invention further found that there is an intermediate phase of tricalcium disilicate between the monocalcium silicate and the dicalcium silicate, which causes the cement clinker of the present invention to solidify, resulting in the formation of hard large particles that are not easy to be ground and increase the grinding energy consumption. For this reason, the present invention adds Li in the preparation of raw materials 2 O source, among which Li 2 O enters the crystal structure of tricalcium disilicate as a catalyst, destroying its structural stability, and then decomposing tricalcium disilicate at 1050°C. Since this temperature is lower than the formation temperature of the target product in the cement clinker of the present invention (1075-1175°C), it is equivalent to eliminating tricalcium disilicate before the target product is formed, preventing it from causing the target product to solidify. At the same time, the Li 2 O also decomposes tricalcium disilicate to form monocalcium silicate and dicalcium silicate, which are the target components of the cement clinker of the present invention. This not only eliminates the cement clinker consolidation problem caused by tricalcium disilicate, but also converts this unfavorable factor into a favorable factor, becoming the target components of the cement clinker of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0020] Figure 1 This is a sample picture of the monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker prepared in the following Example 1.

[0021] Figure 2 The XRD spectrum of the monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker prepared in the following Example 1.

[0022] Figure 3 This is the XRD spectrum of the monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker prepared in the following Example 2.

[0023] Figure 4 This is the XRD spectrum of the monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker prepared in the following Example 3.

[0024] Figure 5 This is the XRD spectrum of the monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker prepared in the following Example 4.

[0025] Figure 6 This is the XRD pattern of the monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker prepared in the following Example 5.

[0026] Figure 7 This is the XRD spectrum of the monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker prepared in the following Example 6.

[0027] Figure 8 This is a sample picture of cement clinker prepared in the following Example 6.

[0028] Fig. 9 This is the XRD spectrum of the monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker prepared in the following Example 7.

[0029] Fig.10 This is a sample picture of cement clinker prepared in the following Example 7. DETAILED DESCRIPTION

[0030] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0031] Unless otherwise defined, all professional and scientific terms used in the present invention have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions.

[0032] In addition, any method and material similar or equivalent to the described content can be applied to the method of the present invention. The technical solution of the present invention is further described in conjunction with the accompanying drawings and specific embodiments.

[0033] In the following embodiments, the limestone is purchased from Shandong Shan Aluminum Environmental New Materials Co., Ltd. The sandstone is purchased from Shandong Shan Aluminum Environmental New Materials Co., Ltd. The silica fume is purchased from Shandong Shan Aluminum Environmental New Materials Co., Ltd. The desulfurized gypsum is purchased from Shandong Shan Aluminum Environmental New Materials Co., Ltd. The fluorinated gypsum is purchased from Shandong Shan Aluminum Environmental New Materials Co., Ltd. The fly ash is purchased from Shandong Shan Aluminum Environmental New Materials Co., Ltd. The lithium slag is purchased from Jiangxi Yichun Yinli New Energy Co., Ltd., and the mass fraction of lithium oxide in the lithium slag is 0.67%.

[0034] Example 1

[0035] 1. A method for preparing monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker, comprising the following steps:

[0036] (1) Take the following raw materials: 70 parts by weight of limestone, 55 parts by weight of sandstone, 28 parts by weight of desulfurized gypsum, 2 parts by weight of lithium slag, and 0.5 parts by weight of calcium fluoride. Grind the above raw materials separately and pass them through a 200-mesh sieve to obtain the powders of the raw materials for later use.

[0037] (2) The raw material powders of step (1) are mixed uniformly according to proportion to obtain cement raw material.

[0038] (3) The cement raw material of step (2) is placed in a furnace and heated to 1075°C at a heating rate of 10°C / min and calcined for 40 minutes. After completion, the calcined product is rapidly cooled by air cooling to obtain cement clinker (such as Figure 1 as shown).

[0039] The cement clinker prepared in this embodiment was subjected to XRD test (eg Figure 2 The results show that the mineral composition of the clinker prepared in this embodiment includes: calcium silicate (CS) with a content of 11.96%, calcium sulfosilicate (C 5 S 2 $) content is 44.92%, dicalcium silicate (C 2 S) content is 36.02%, and the content of grosvenorite (C 2 AS) content is 1.06%, glass phase 3.87%, and the remainder is unreacted raw materials and inevitable impurities (such as SiO 2 、CaSO 4 , Li 6 O 7 Si 2 wait).

[0040] Figure 1The sample of the cement clinker prepared in this embodiment can be seen to be in a clearly loose state. The particles therein are formed by the continuous rolling of the clinker during the firing process in the cement rotary kiln and are also in a very loose state. Such clinker is easier to grind and requires less energy consumption.

[0041] 2. A preparation of a monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement composition comprises the following steps: 94 parts by weight of the monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker prepared in this embodiment and 5 parts by weight of gypsum powder are taken, the cement clinker and gypsum powder are mixed and then ground to obtain the cement composition.

[0042] Example 2

[0043] 1. A method for preparing monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker, comprising the following steps:

[0044] (1) Take the following raw materials: 80 parts by weight of limestone, 65 parts by weight of silica fume, 38 parts by weight of desulfurized gypsum, 1.5 parts by weight of lithium slag, and 0.6 parts by weight of calcium fluoride. Grind the above raw materials separately and pass them through a 200-mesh sieve to obtain the powders of the raw materials for later use.

[0045] (2) The raw material powders of step (1) are mixed uniformly according to proportion to obtain cement raw material.

[0046] (3) The cement raw material of step (2) is placed in a furnace and heated to 1125° C. at a heating rate of 10° C. / min and calcined for 30 min. After completion, the calcined product is rapidly cooled by air cooling to obtain cement clinker.

[0047] The cement clinker prepared in this embodiment was subjected to XRD test (eg Figure 3 The results show that the mineral composition of the clinker prepared in this embodiment includes: calcium silicate (CS) with a content of 11.72%, calcium sulfosilicate (C 5 S 2 $) content is 27.03%, dicalcium silicate (C 2 S) content is 54.97%, and the content of grosvenorite (C 2 AS) content is 2.91%, glass phase 1.36%, and the balance is unreacted raw materials and unavoidable impurities (such as SiO 2 、CaSO 4 , Li 6 O 7 Si 2 wait).

[0048] 2. A preparation of a monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement composition, comprising the following steps: taking 95 parts by weight of the monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker prepared in this embodiment and 5 parts by weight of gypsum powder, mixing the cement clinker and gypsum powder uniformly and then grinding them to obtain the cement composition.

[0049] Example 3

[0050] A method for preparing monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker comprises the following steps:

[0051] (1) Take the following raw materials: 65 parts by weight of limestone, 43 parts by weight of sandstone, 22 parts by weight of fluorgypsum, 0.5 parts by weight of lithium slag, and 0.1 parts by weight of calcium fluoride. Grind the above raw materials separately and pass them through a 200-mesh sieve to obtain the powders of the raw materials for later use.

[0052] (2) The raw material powders of step (1) are mixed uniformly according to proportion to obtain cement raw material.

[0053] (3) The cement raw material of step (2) is placed in a furnace and heated to 1125° C. at a heating rate of 10° C. / min and calcined for 30 min. After completion, the calcined product is rapidly cooled by air cooling to obtain cement clinker.

[0054] The cement clinker prepared in this embodiment was subjected to XRD test (eg Figure 4 The results show that the mineral composition of the clinker prepared in this embodiment includes: calcium silicate (CS) with a content of 6.21%, calcium sulfosilicate (C 5 S 2 $) content is 30.47%, dicalcium silicate (C 2 S) content is 54.79%, and the content of grosvenorite (C 2 AS) content is 3.02%, glass phase 3.95%, and the balance is unreacted raw materials and inevitable impurities (such as SiO 2 、CaSO 4 , Li 6 O 7 Si 2 wait).

[0055] 2. A preparation of a monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement composition comprises the following steps: 98 parts by weight of the monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker prepared in this embodiment and 3 parts by weight of gypsum powder are taken, the cement clinker and gypsum powder are mixed and then ground to obtain the cement composition.

[0056] Example 4

[0057] A method for preparing monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker comprises the following steps:

[0058] (1) Take the following raw materials: 70 parts by weight of carbide slag, 65 parts by weight of coal gangue, 38 parts by weight of fluorgypsum, 2 parts by weight of lithium slag, and 1 part by weight of calcium fluoride. Grind the raw materials separately and pass them through a 200-mesh sieve to obtain the powders of the raw materials for later use.

[0059] (2) The raw material powders of step (1) are mixed uniformly according to proportion to obtain cement raw material.

[0060] (3) The cement raw material of step (2) is placed in a furnace and heated to 1150° C. at a heating rate of 10° C. / min and calcined for 10 min. After completion, the calcined product is rapidly cooled by air cooling to obtain cement clinker.

[0061] The cement clinker prepared in this embodiment was subjected to XRD test (eg Figure 5 The results show that the mineral composition of the clinker prepared in this embodiment includes: calcium silicate (CS) content of 6.06%, calcium sulfosilicate (C 5 S 2 $) content is 44.79%, dicalcium silicate (C 2 S) content is 44.13%, and the content of grosvenorite (C 2 AS) content is 0.48%, glass phase 1.01%, and the balance is unreacted raw materials and inevitable impurities (such as SiO 2 、CaSO 4 , Li 6 O 7 Si 2 wait).

[0062] 2. A preparation of a monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement composition comprises the following steps: 92 parts by weight of the monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker prepared in this embodiment and 4 parts by weight of gypsum powder are taken, the cement clinker and gypsum powder are mixed and then ground to obtain the cement composition.

[0063] Example 5

[0064] A method for preparing monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker comprises the following steps:

[0065] (1) Take the following raw materials: 75 parts by weight of quicklime, 65 parts by weight of sandstone, 22 parts by weight of phosphogypsum, 1.8 parts by weight of lithium slag, and 1 part by weight of calcium fluoride. Grind the above raw materials separately and pass them through a 200-mesh sieve to obtain the powders of the raw materials for later use.

[0066] (2) The raw material powders of step (1) are mixed uniformly according to proportion to obtain cement raw material.

[0067] (3) The cement raw material of step (2) is placed in a furnace and heated to 1175° C. at a heating rate of 10° C. / min and calcined for 10 min. After completion, the calcined product is rapidly cooled by air cooling to obtain cement clinker.

[0068] The cement clinker prepared in this embodiment was subjected to XRD test (eg Figure 6 The results show that the mineral composition of the clinker prepared in this embodiment includes: calcium silicate (CS) with a content of 8.41%, calcium sulfosilicate (C 5 S 2 $) content is 45.07%, dicalcium silicate (C 2 S) content is 36.32%, and the content of grosvenorite (C 2 AS) content is 2.77%, glass phase 4.03%, and the balance is unreacted raw materials and inevitable impurities (such as SiO 2 、CaSO 4 , Li 6 O 7 Si 2 wait).

[0069] 2. A preparation of a monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement composition comprises the following steps: 97 parts by weight of the monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker prepared in this embodiment and 3 parts by weight of gypsum powder are taken, the cement clinker and gypsum powder are mixed and then ground to obtain the cement composition.

[0070] Example 6

[0071] A method for preparing cement clinker comprises the following steps:

[0072] (1) Take the following raw materials: 80 parts by weight of limestone, 65 parts by weight of silica fume, 38 parts by weight of desulfurized gypsum, and 0.6 parts by weight of calcium fluoride. Grind the above raw materials separately and pass them through a 200-mesh sieve to obtain the powders of the raw materials for later use.

[0073] (2) The raw material powders of step (1) are mixed uniformly according to proportion to obtain cement raw material.

[0074] (3) The cement raw material of step (2) is placed in a furnace and heated to 1125° C. at a heating rate of 10° C. / min and calcined for 30 min. After completion, the calcined product is rapidly cooled by air cooling to obtain cement clinker.

[0075] The cement clinker prepared in this embodiment was subjected to XRD test (eg Figure 7 The results show that the mineral composition of the clinker prepared in this embodiment includes: calcium sulfosilicate (C 5 S 2 $) content is 24.65%, dicalcium silicate (C 2 S) content is 47.17%, tricalcium disilicate (C 3 S 2 ) content is 15.72%, calcite (C 2 AS) content is 5.32%, glass phase 4.54%, and the balance is unreacted raw materials and unavoidable impurities (such as SiO 2 、CaSO 4 It can be seen that due to the absence of Li 2 O source, the cement clinker prepared in this embodiment contains a large amount of tricalcium disilicate, which is easy to cause the clinker to solidify. Figure 8 It can be seen from the cement clinker prepared in this embodiment that the cement clinker has a serious solidification phenomenon, which makes the clinker difficult to grind and requires more grinding energy.

[0076] Example 7

[0077] A method for preparing cement clinker comprises the following steps:

[0078] (1) Take the following raw materials: 70 parts by weight of carbide slag, 65 parts by weight of coal gangue, 38 parts by weight of fluorgypsum, and 1 part by weight of calcium fluoride. Grind the above raw materials separately and pass them through a 200-mesh sieve to obtain the powders of the raw materials for later use.

[0079] (2) The raw material powders of step (1) are mixed uniformly according to proportion to obtain cement raw material.

[0080] (3) The cement raw material of step (2) is placed in a furnace and heated to 1150° C. at a heating rate of 10° C. / min and calcined for 10 min. After completion, the calcined product is rapidly cooled by air cooling to obtain cement clinker.

[0081] The cement clinker prepared in this embodiment was subjected to XRD test (eg Fig. 9 The results show that the mineral composition of the clinker prepared in this embodiment includes: calcium sulfosilicate (C 5 S 2 $) content is 32.65%, dicalcium silicate (C 2 S) content is 33.78%, tricalcium disilicate (C 3 S2 ) content is 22.14%, calcite (C 2 AS) content is 5.41%, glass phase 3.14%, and the remainder is unreacted raw materials and inevitable impurities (such as SiO 2 、CaSO 4 It can be seen that due to the absence of Li 2 O source, the cement clinker prepared in this embodiment contains a large amount of tricalcium disilicate, which is easy to cause the clinker to solidify. Fig.10 It can be seen from the cement clinker prepared in this embodiment that the cement clinker has a serious solidification phenomenon, which makes the clinker difficult to grind and requires more grinding energy.

[0082] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A calcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker, characterized in that: include: Monocalcium silicate 6~12wt.%, calcium sulfosilicate 27~45wt.%, dicalcium silicate 36~55wt.%, grossamite 0.48~3wt.%, glass phase 1~4wt.%, and the remainder are unreacted raw materials and unavoidable impurities.

2. The method for preparing monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker according to claim 1, characterized in that: The steps include: (1) Take the following raw materials: 65-80 parts by weight of calcium raw material, 43-65 parts by weight of silicon raw material, 22-38 parts by weight of gypsum, 0.5-2 parts by weight of Li2O source, and 0.1-1 parts by weight of calcium fluoride; (2) calcining the powdered raw material formed by the above raw materials at a temperature not higher than 1200° C., quenching the raw material after calcination, and then grinding the raw material to obtain the cement clinker; In step (1), the Li2O source includes at least one of lithium slag, carbonate clay-type lithium ore, and volcanic clay-type lithium ore; and the mass fraction of Li2O in the Li2O source is not less than 0.5%.

3. The method for preparing monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker according to claim 2, characterized in that: In step (1), the calcium raw material includes at least one of limestone, carbide slag, quicklime and high-calcium fly ash.

4. The method for preparing monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker according to claim 2, characterized in that: In step (1), the siliceous raw material includes at least one of sandstone, stripping soil, silica ash and coal gangue.

5. The method for preparing monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker according to claim 2, characterized in that: In step (1), the gypsum includes at least one of desulfurized gypsum, fluorinated gypsum, phosphogypsum, borogypsum and titanium gypsum.

6. The method for preparing monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker according to any one of claims 2 to 5, characterized in that: In step (2), the calcination temperature is 1075~1175°C.

7. The method for preparing monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker according to claim 6, characterized in that: In step (2), the calcination time is 10 to 40 minutes.

8. A calcium silicate-calcium sulfosilicate-dicalcium silicate cement composition, characterized in that: include: 92-98 parts by weight of the monocalcium silicate-calcium sulfosilicate-dicalcium silicate cement clinker according to claim 1 or the cement clinker obtained by the preparation method according to any one of claims 2-7, and 3-5 parts by weight of gypsum.

Citation Information

Patent Citations

  • Modified sulphoaluminate cement and preparation method and application thereof

    CN112608047A

  • Carbonizable low-carbon cement clinker as well as preparation method and application thereof

    CN117401916A

  • Carbonation hardened low-calcium cement and preparation and hardening method thereof

    CN117645420A

  • All-solid-waste low-carbon type ternary mineral gelling system and preparation method thereof

    CN117865522A

  • Method for preparing calcium sulphosilicate-dicalcium silicate-calcium sulphoaluminate system from calcium carbide slag and method for improving late-stage

    GB202203020D0