Flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder and preparation process thereof

By pre-treating the porous structure of shell powder and sand and combining it with nano-cerium oxide, the problem of insufficient adsorption capacity and compatibility of shell powder is solved, forming an efficient porous structure and improving the freshness, waterproofing and flame retardancy of polypropylene plastic storage boxes. performance, extending the shelf life of food and the service life of plastic boxes.

CN118480229BActive Publication Date: 2024-10-29SHANDONG RUICHI MAN ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410529203.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-29
Publication Date
2024-10-29
Estimated Expiration
2044-04-29

AI Technical Summary

Technical Problem

Shell powder has limited adsorption capacity and poor compatibility with polypropylene plastic, causing delamination and cracking of plastic boxes, affecting performance and lifespan; sand easily absorbs water and moisture, causing food to become damp and spoilage, shortening the shelf life.

Method used

The pretreated shell powder is calcined at high temperature to form a porous structure, added to the plastic preservation box, and mixed with the cerium source and organic intercalation agent for hydrothermal treatment to form a cerium carbonate layer and nano-cerium oxide; the sand is carbonized at high temperature to form porous carbon, which is adsorbed dirt and moisture, and mixed with antioxidants to improve stability; porous carbon-loaded sand is cross-linked with cellulose nanofibers to form a highly efficient aerogel structure.

Benefits of technology

It improves the thermal insulation performance, antioxidant and fresh-keeping effects of the fresh-keeping box, extends the shelf life of food, enhances the waterproof and flame-retardant properties of the plastic box, and improves the service life and storage effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder and a preparation process thereof, which belongs to the technical field of plastic fresh-keeping box preparation, and comprises the following raw materials by weight: 80-100 parts of polypropylene, 40-60 parts of modified calcined shell powder, 41-49 parts of silica sol, 40-50 parts of expanded perlite, 10-20 parts of sand-based composite aerogel, 5-10 parts of coupling agent, 2-3 parts of dispersant, 3-5 parts of plasticizer, and 0.01-0.03 parts of flame retardant. A cerium carbonate layer is formed between the calcined shell powder layers, showing good barrier properties, and can effectively prevent the penetration of moisture, oxygen and other harmful substances; the excellent adsorption of porous carbon can adsorb and fix metal elements such as aluminum and iron in the sand to avoid affecting the performance of the fresh-keeping box.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plastic fresh-keeping box preparation, in particular to a flame-retardant polypropylene plastic fresh-keeping box added with sand and calcined shell powder and a preparation process thereof. Background Art

[0002] Polypropylene is a semi-crystalline thermoplastic with high impact resistance, toughness, solvent resistance, acid and alkali corrosion resistance, and has the advantages of being non-toxic, odorless, and inexpensive. It is widely used as a fresh-keeping box for long-distance transportation of fruits. Fresh-keeping boxes are divided into plastic fresh-keeping boxes, foam fresh-keeping boxes, and technological fresh-keeping boxes. Plastic fresh-keeping boxes are made of resin materials. Polypropylene fresh-keeping boxes are safe and harmless to the human body. They are widely used for their small specific gravity, easy processing, and non-toxicity. Polypropylene fresh-keeping boxes are made of polypropylene resin, aggregates, and additives through a twin-screw extruder, granulated, and the granules are pressed to form a composite sheet. The composite sheet is then die-cut and printed to obtain a polypropylene plastic fresh-keeping box.

[0003] Shell powder has excellent adsorption properties. As the aggregate of polypropylene plastic fresh-keeping boxes, it can remove odors and moisture in the fresh-keeping boxes, extend the shelf life of food, and reduce food spoilage. However, the adsorption capacity of shell powder is limited, and the compatibility between shell powder and polypropylene plastic is poor. It is easy to precipitate, causing problems such as stratification and cracking of the plastic box, affecting the performance and life of the plastic box. Sand particles contain strong hydrophilic groups, which are easy to absorb water and moisture, causing the food in the polypropylene plastic fresh-keeping box to become damp and spoil, shortening the shelf life of food and affecting the quality and taste of food. Therefore, the polypropylene fresh-keeping box should also have good waterproof properties. Summary of the invention

[0004] The purpose of the present invention is to provide a flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder and a preparation process thereof: the shell powder is pretreated and calcined at high temperature to form a shell powder with a large specific surface area and a porous structure, which is added to the plastic fresh-keeping box to absorb odors, mixed with a cerium source and an organic intercalant, and then subjected to hydrothermal treatment to form a cerium carbonate layer between the calcined shell powder layers, showing good barrier properties, and the cerium source can also form nano-cerium oxide in the pores of the calcined shell powder, which refines the pore size of the shell powder, so that the shell powder has a lower thermal conductivity, thereby improving the thermal insulation performance, anti-oxidation and fresh-keeping effects of the fresh-keeping box; the sand is washed and dried After drying, it is mixed with a carbon precursor and a connector, and carbonized at high temperature to synthesize porous carbon on the surface of the sand, which can absorb more dirt and moisture on the surface of the polypropylene plastic fresh-keeping box, and the porous carbon can adsorb and fix metal elements such as aluminum and iron in the sand to avoid affecting the performance of the fresh-keeping box; the sand loaded with porous carbon is mixed with an antioxidant, and the antioxidant is coated on the porous carbon. The porous carbon serves as a carrier to improve the stability of the antioxidant in the plastic fresh-keeping box, and is added to cellulose nanofibers and melamine formaldehyde resin for cross-linking. After freeze-drying, the sand increases the cross-linking density of the aerogel, reduces the pore size and increases the porosity, thereby improving the mechanical properties of the aerogel.

[0005] The technical problem to be solved by the present invention is as follows: shell powder can remove odor and moisture in a fresh-keeping box, extend the shelf life of food, and reduce food spoilage, but the adsorption capacity of shell powder is limited, and the compatibility between shell powder and polypropylene plastic is poor, and shell powder is easy to precipitate, causing problems such as stratification and cracking of the plastic box, affecting the performance and life of the plastic box; sand particles contain strong hydrophilic groups, which are easy to absorb water and moisture, causing the food in the polypropylene plastic fresh-keeping box to become damp and spoil, shortening the shelf life of food, and affecting the quality and taste of food.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder comprises the following raw materials in parts by mass: 80-100 parts of polypropylene, 40-60 parts of modified calcined shell powder, 41-49 parts of silica sol, 40-50 parts of expanded perlite, 10-20 parts of sand-based composite aerogel, 5-10 parts of coupling agent, 2-3 parts of dispersant, 3-5 parts of plasticizer and 0.01-0.03 parts of flame retardant.

[0008] A preparation process of a flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder, comprising the following steps:

[0009] S1. Add the modified calcined shell powder to the silica sol, stir evenly, add 60% by mass hydrochloric acid to adjust the pH to 2.5, stir for 25 minutes, add 36% by mass ammonia water to adjust the pH to 7, add expanded perlite, evacuate to -0.04MPa, take out after adsorption, place in anhydrous ethanol for aging, and dry to obtain a solid.

[0010] Among them, the hydroxyl groups contained on the surface of the modified calcined shell powder can be combined with the hydroxyl groups produced by the hydrolysis of silica sol through chemical bonds, so that the modified calcined shell powder can be filled into the silicone gel system, and the silicone gel can be filled into the pores of the expanded perlite, gelled in the pores, and the pore size of the expanded perlite is refined, so that the pore size of the expanded perlite is transformed from macropores to mesoporous structures, thereby increasing the porosity, and improving the thermal insulation and air permeability of the fresh-keeping box. In addition, methyltriethoxysilane in the silicone gel loaded with expanded perlite shows excellent hydrophobicity and has good waterproof performance.

[0011] S2. Mix polypropylene, the solid prepared in step S1, the sand-based composite aerogel, the coupling agent, the dispersant, the plasticizer, and the flame retardant, stir, place in a twin-screw extruder, extrude and granulate, place the granules in a mold, press to form a composite board, and then die-cut and print to obtain a polypropylene plastic fresh-keeping box.

[0012] Furthermore, the expanded perlite has a particle size of 0.5-0.8 mm and a pore size of 40-50 μm.

[0013] More preferably, the expanded perlite has a particle size of 0.6 mm and a pore size of 45 μm.

[0014] Furthermore, the coupling agent is selected from vinyltrimethoxysilane or zirconate coupling agent.

[0015] Furthermore, the plasticizer is selected from stearic acid or dibutyl phthalate.

[0016] Furthermore, the dispersant is selected from paraffin or cyclohexanol.

[0017] Furthermore, the flame retardant is selected from any one of decabromodiphenylethane, brominated epoxy resin, and brominated polystyrene.

[0018] Furthermore, the temperature of the first section of the twin-screw extruder is 170-180°C, the temperature of the second section is 185-195°C, and the temperature of the third section is 210-220°C; the rotation speed is 130-150rpm, and the aspect ratio of the twin-screw extruder is 18-22:0.5-1.5.

[0019] More preferably, the temperature of the first section of the twin-screw extruder is 175° C., the temperature of the second section is 190° C., and the temperature of the third section is 215° C.; the rotation speed is 140 rpm, and the aspect ratio of the twin-screw extruder is 20:1.

[0020] Furthermore, the modified calcined shell powder is prepared by calcining the pretreated shell powder at high temperature, mixing it with a cerium source and an organic intercalation agent, and then subjecting it to hydrothermal treatment.

[0021] Furthermore, the high temperature calcination temperature is 800-1100° C., and the high temperature calcination time is 2-4 hours.

[0022] More preferably, the high temperature calcination temperature is 800-1000° C., and the high temperature calcination time is 2-3 h.

[0023] More preferably, the high temperature calcination temperature is 900° C. and the high temperature calcination time is 2.5 h.

[0024] Furthermore, the organic intercalant is selected from any one of tetrabutylammonium bromide, hexadecyltrimethylammonium bromide, dodecyltrimethylammonium bromide and sodium diethylphosphinate.

[0025] Furthermore, the cerium source is selected from cerium nitrate hexahydrate, cerium chloride, and cerium sulfate.

[0026] More preferably, the cerium source is selected from cerium nitrate hexahydrate and cerium chloride.

[0027] Further preferably, the cerium source is selected from cerium nitrate hexahydrate.

[0028] Furthermore, the hydrothermal treatment temperature is 200-250°C, and the hydrothermal treatment time is 8-10h.

[0029] More preferably, the hydrothermal treatment temperature is 230° C. and the hydrothermal treatment time is 9 h.

[0030] Further, the modified calcined shell powder is prepared by the following steps:

[0031] The pretreated shell powder was placed in a muffle furnace, calcined at 900°C for 2.5 hours, and then cooled to room temperature to obtain calcined shell powder. The calcined shell powder was added to deionized water, stirred evenly, and an organic intercalation agent and a cerium source were added. The mixture was stirred at 80°C for 30 minutes, placed in a reactor, heated to 230°C, and subjected to hydrothermal reaction for 9 hours. The mixture was cooled to room temperature, filtered, washed with deionized water for 3 times, and dried in an oven at 85°C for 15 minutes to obtain modified calcined shell powder.

[0032] Among them, after the pretreated shell powder is calcined at high temperature, the organic matter between the shell powder layers is decomposed by heat to form shell powder with a layered structure, and the main component of the shell powder, calcium carbonate, is decomposed by heat to form calcium oxide and carbon dioxide. The pretreated shell powder has a large specific surface area and a porous structure, which can absorb odors when added to a plastic fresh-keeping box.

[0033] Furthermore, the organic intercalant can exchange calcium ions with the layered shell powder layers, so that the organic intercalant is intercalated into the layers of the calcined shell powder, expanding the interlayer spacing of the shell powder and increasing the adsorption capacity of the shell powder. Under the action of the intercalant, the cerium ions in the cerium source can more easily enter the intercalated shell powder layers, and the carbonate ions contained in the interlayers can combine with the cerium ions, thereby forming a cerium carbonate layer between the layers of the shell powder, showing better barrier properties.

[0034] In addition, the cerium source can be filled into the pores of the shell powder after intercalation with the intercalant. After hydrothermal treatment, the cerium ions combine with oxygen atoms to form cerium oxide crystals. The cerium oxide crystals nucleate and grow, and nano-cerium oxide is formed in the pores of the shell powder. The pore size of the shell powder is refined, and the shell powder has a lower thermal conductivity, thereby improving the thermal insulation performance, anti-oxidation and preservation effects of the fresh-keeping box.

[0035] Furthermore, the pore size of the calcined shell powder is 80-100 nm; the particle size is 6.5-13 μm.

[0036] Furthermore, the mass ratio of the calcined shell powder, deionized water, organic intercalation agent and cerium source is 2-3:70-90:3-4:0.3-0.5.

[0037] Furthermore, the pre-treated shell powder is prepared by washing the shell powder, grinding it into powder, sieving it, and treating it with an alkali agent.

[0038] Furthermore, the alkaline treatment agent is selected from one of sodium hydroxide solution and potassium hydroxide solution.

[0039] Further preferably, the alkaline treatment agent is selected from sodium hydroxide solution.

[0040] Furthermore, the concentration of the alkali treatment agent sodium hydroxide solution is 1.2-3.5 mol / L.

[0041] More preferably, the concentration of the alkali treatment agent sodium hydroxide solution is 2.5 mol / L.

[0042] Furthermore, the sieve mesh has an aperture of 1000-2000 mesh.

[0043] Further, the pretreated shell powder is specifically prepared by the following steps:

[0044] The shell powder was washed with deionized water for 5 times to clean the surface impurities, and dried in a 65°C forced air drying oven for 10 minutes. The dried shell powder was placed in a grinder and crushed for 10 minutes. The powder was passed through a 1500-mesh sieve and placed in a 2.5 mol / L alkaline treatment agent sodium hydroxide solution, stirred for 30 minutes, filtered and washed with deionized water for 3 times, and dried in a 70°C oven for 10 minutes to obtain the pretreated shell powder.

[0045] The shell powder is washed and dried to remove impurities on the surface of the shell powder, and then treated with an alkaline treatment agent, sodium hydroxide solution. The sodium hydroxide can chemically react with lipids in the pores of the shell powder to expose more pores and improve the adsorption performance.

[0046] Furthermore, the usage ratio of shell powder and alkali treatment agent is 3-7g:45-55mL.

[0047] Furthermore, the sand-based composite aerogel is prepared by mixing porous carbon-loaded sand with an antioxidant, adding the mixture to cellulose nanofibers and melamine formaldehyde resin for cross-linking, and then freeze-drying.

[0048] Furthermore, the antioxidant is selected from any one of tocopherol, butylated hydroxytoluene and ascorbic acid.

[0049] Furthermore, the cellulose nanofibers have a length of 2-10 μm and a diameter of 10-50 nm.

[0050] More preferably, the cellulose nanofibers have a length of 2-8 μm and a diameter of 10-40 nm.

[0051] More preferably, the cellulose nanofibers have a length of 4.5 μm and a diameter of 30 nm.

[0052] Furthermore, the freeze-drying temperature is -(20-40)°C, and the freeze-drying time is 1-3h.

[0053] More preferably, the freeze-drying temperature is -30°C and the freeze-drying time is 2 hours.

[0054] Further, the sand-based composite aerogel is specifically prepared by the following steps:

[0055] Add antioxidant to ethanol and stir evenly, add sand loaded with porous carbon, place in a sealed container, and after adsorption at -0.04MPa, heat at 85°C until the organic solvent evaporates to obtain a solid, add melamine formaldehyde resin and cellulose nanofibers to deionized water, stir at 1500r / min for 5h to make them evenly dispersed, add 0.2mL of 4M hydrochloric acid solution to adjust the pH to 0.1, add methyltrimethoxysilane and solid, stir the reaction for 2h, and freeze-dry at -30°C for 2h to obtain a sand-based composite aerogel.

[0056] Among them, the sand loaded with porous carbon adsorbs the antioxidant, so that the antioxidant is coated on the porous carbon. The porous carbon serves as a carrier, which improves the stability of the antioxidant in the plastic fresh-keeping box and avoids the migration and precipitation of the antioxidant.

[0057] Furthermore, the cellulose nanofibers serve as an aerogel skeleton, and the hydroxyl and carboxyl groups on their surfaces can react with the amino groups on the molecular chains of the melamine formaldehyde resin. Under the action of the cross-linking agent methyltrimethoxysilane, a porous aerogel structure with a cross-linked network structure is formed. The hydroxyl groups on the surface of the sand loaded with porous carbon adsorbed with antioxidants can be chemically bonded to the oxygen-containing functional groups in the porous aerogel with a cross-linked network structure, so that the sand loaded with antioxidants is embedded in the composite aerogel, increasing the cross-linking density, reducing the pore size and increasing the porosity, thereby improving the mechanical properties of the aerogel. In addition, the sand loaded with porous carbon is chemically bonded to the cellulose nanofiber aerogel, thereby improving the heat resistance of the fiber aerogel, preventing the cellulose from being easily decomposed by heat, and improving the thermal stability of the fresh-keeping box.

[0058] Furthermore, the mass ratio of the antioxidant, the porous carbon-loaded sand, the melamine formaldehyde resin, the cellulose nanofiber, and the deionized water is 3-4 g: 4-5 g: 0.4-0.5 g: 0.3-0.7 g.

[0059] Furthermore, the porous carbon-loaded sand is prepared by washing and drying the sand, mixing it with a carbon precursor and a connecting agent, and then carbonizing it at a high temperature.

[0060] Furthermore, the carbon precursor is selected from one of glucose, rice husk powder, starch and bagasse.

[0061] More preferably, the carbon precursor is selected from one of glucose and rice husk powder.

[0062] More preferably, the carbon precursor is selected from one of glucose.

[0063] Furthermore, the high temperature carbonization temperature is 750-950°C, and the high temperature carbonization time is 1-4h.

[0064] More preferably, the high-temperature carbonization temperature is 800° C. and the high-temperature carbonization time is 3 h.

[0065] Furthermore, the linking agent is selected from any one of citric acid, ethylene glycol, and oxalic acid.

[0066] Further, the porous carbon-loaded sand is prepared by the following steps:

[0067] The sand was washed with deionized water to remove surface impurities, dried in an oven at 70°C, placed in ethanol, added with a carbon precursor and a connector, stirred evenly, added with 36% hydrochloric acid by mass, stirred and reacted at 70°C for 30 minutes, filtered, washed, and dried, placed in a tubular furnace, activated with potassium hydroxide, introduced with nitrogen, carbonized at 800°C for 3 hours, cooled to room temperature, taken out, washed with deionized water until the washing liquid was neutral, and dried in an oven at 70°C for 10 minutes to obtain sand loaded with porous carbon.

[0068] The sand is washed and dried to remove surface impurities and dirt, and the hydroxyl groups on the surface of the pure sand can be chemically bonded with the oxygen-containing functional groups in the carbon precursor, and citric acid is used as a linker to coat the carbon precursor on the surface of the sand. After high-temperature carbonization, the carbon precursor is decomposed by heat to form a dense carbon layer, and the activator potassium hydroxide molecules are decomposed to form pores on the surface of the dense carbon layer, thereby realizing the synthesis of porous carbon on the surface of the sand. The synthesized porous carbon has high adsorption properties and can adsorb more dirt and moisture on the surface of the polypropylene plastic fresh-keeping box.

[0069] Furthermore, the mass ratio of sand, carbon precursor and connecting agent is 1.6-2:4-6:0.2-0.3.

[0070] Furthermore, compared with the prior art, the present invention has the following beneficial effects:

[0071] (1) In the technical scheme of the present invention, after the pre-treated shell powder is calcined at high temperature, a layered shell powder is formed, which has an ion exchange function, and the main component of the shell powder, calcium carbonate, is decomposed by heat to form calcium oxide and carbon dioxide, so that the shell powder has a large specific surface area and a porous structure, which can be added to the plastic fresh-keeping box to absorb odor; the organic intercalating agent is intercalated between the layers of the calcined shell powder to expand the interlayer spacing of the shell powder, increase the adsorption capacity of the shell powder, and more efficiently remove the odor and moisture in the fresh-keeping box, thereby extending the shelf life of food and reducing food corruption; under the action of the intercalating agent, the cerium ions in the cerium source can more easily enter the intercalated shell powder layers, and a cerium carbonate layer is formed between the calcined shell powder layers, which exhibits good barrier properties and can effectively prevent the penetration of moisture, oxygen and other harmful substances, and prevent the stored items from being affected by moisture and oxidation factors, thereby extending the shelf life of the items; the formed cerium carbonate can absorb ultraviolet rays, reduce ultraviolet light aging, and make the fresh-keeping box still have a good storage effect under light;

[0072] (2) In the technical solution of the present invention, the nano-cerium oxide formed by the cerium source in the pores of the calcined shell powder refines the pore size of the shell powder, so that the shell powder has a lower thermal conductivity, thereby improving the thermal insulation performance, anti-oxidation and preservation effect of the fresh-keeping box. The nano-cerium oxide also has anti-oxidation and corrosion resistance, thereby extending the service life of the fresh-keeping plastic;

[0073] (3) In the technical scheme of the present invention, the shell powder loaded with nanoparticles is filled into the silicone gel system, and the silicone gel can be filled into the pores of the expanded perlite and gelled in the pores of the expanded perlite. On the one hand, the pore size of the expanded perlite is refined, so that the pore size of the expanded perlite is converted from a macroporous structure to a mesoporous structure, thereby increasing the porosity, improving the thermal insulation and air permeability of the fresh-keeping box, and the expanded perlite is also used as a fireproof material to provide flame retardant properties for the fresh-keeping box. On the other hand, the methyltriethoxysilane contained in the silicone gel in the pores of the expanded perlite is combined with the hydrophilic hydroxyl groups on the surface of the silicone gel, showing excellent hydrophobicity and good waterproof performance, and having good compatibility with the polypropylene plastic matrix, thereby improving the dispersibility of the shell powder in the polypropylene plastic matrix. In addition, the use of the expanded perlite as a carrier can avoid the shedding and agglomeration of the shell powder loaded with nanoparticles, thereby increasing the service life of the plastic safe.

[0074] (4) In the technical scheme of the present invention, porous carbon is synthesized on the surface of sand. The synthesized porous carbon has high adsorption performance and can absorb more dirt and moisture on the surface of the polypropylene plastic fresh-keeping box. The excellent adsorption of porous carbon can adsorb and fix metal elements such as aluminum and iron in the sand to avoid affecting the performance of the fresh-keeping box. The antioxidant can reduce the oxygen content of the food-packaging system, first react with oxygen, remove active oxygen such as singlet oxygen, superoxide free radicals and hydroxyl free radicals in fruits and vegetables, and avoid oxidation of substances in food to achieve antioxidant and fresh-keeping effects. The sand loaded with porous carbon is used to adsorb the antioxidant, so that the antioxidant is coated on the porous carbon. The porous carbon is used as a carrier to improve the stability of the antioxidant in the plastic fresh-keeping box and avoid the migration and precipitation of the antioxidant. The pore size and high porosity of the porous carbon help to reduce the adsorption and diffusion of water molecules inside the porous carbon, thereby improving its hydrophobic performance.

[0075] (5) In the technical scheme of the present invention, cellulose nanofibers are used as the skeleton of aerogels. Under the action of melamine formaldehyde resin and methyltrimethoxysilane, a porous aerogel structure with a cross-linked network structure is formed. Sand loaded with antioxidants is embedded in the composite aerogel, which increases the cross-linking density, reduces the pore size and increases the porosity, thereby improving the mechanical properties of the aerogel. In addition, the sand loaded with porous carbon is chemically bonded to the cellulose nanofiber aerogel, thereby improving the heat resistance of the fiber aerogel, preventing cellulose from being easily decomposed by heat, and improving the thermal stability of the fresh-keeping box. The melamine formaldehyde resin in the composite aerogel can produce a large amount of non-flammable gas during combustion and dilute the flammable gas during combustion, thereby showing excellent flame retardant properties and having a synergistic effect with the flame retardant in the plastic fresh-keeping box. DETAILED DESCRIPTION

[0076] The technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0077] The raw materials used in the embodiments of the present invention are as follows: polypropylene (brand: Z-1500, brand: Shandong Dawn, purchased from Shandong Dawn Polymer Materials Co., Ltd.); hexadecyltrimethylammonium bromide (model 57-09-0, purity 99.2%); cerium nitrate hexahydrate (model 10294-41-4, purity 99.5%); glucose (purity 99%, model 50-99-7); potassium hydroxide (model 1310-58-3, mass fraction is 10.5%); citric acid (model 5949-29-1, purity 99%); tocopherol (model 119-13-1, purity 98.2%); melamine formaldehyde resin (model 3089-11-0, purity 96.2%); methyltrimethoxysilane (manufacturer: Tianjin Damao Chemical Reagent Factory, China, analytical grade); vinyltrimethoxysilane (model 2768-02-7, effective substance 99.3).

[0078] Example 1 The modified calcined shell powder is prepared by the following steps:

[0079] A1. Wash 5g of shell powder with deionized water 5 times to clean the surface impurities, put it in a 65°C blast drying oven and dry it for 10 minutes, put the dried shell powder in a grinder, crush it for 10 minutes, pass it through a 1500-mesh sieve, put it in 50mL of 2.5mol / L sodium hydroxide solution, stir it for 30 minutes, filter it, wash it with deionized water 3 times, and dry it in a 70°C oven for 10 minutes to obtain pretreated shell powder;

[0080] A2. Place the pretreated shell powder in a muffle furnace, calcine it at 900°C for 2.5 hours, and then cool it to room temperature to obtain calcined shell powder. Add 2.5g of the calcined shell powder into 80mL of deionized water, stir evenly, add 3.5g of hexadecyltrimethylammonium bromide and 0.43g of cerium nitrate hexahydrate, stir at 80°C for 30 minutes, place it in a reactor, heat it to 230°C, carry out hydrothermal reaction for 9 hours, cool it to room temperature, filter it, wash it with deionized water 3 times, and dry it in an oven at 85°C for 15 minutes to obtain modified calcined shell powder.

[0081] The difference between this comparative example and Example 1 is that cerium nitrate hexahydrate is not added, and the remaining steps and raw materials are the same as those of Example 1.

[0082] Wash 5g of shell powder with deionized water for 5 times, put it in a 65℃ forced air drying oven and dry it for 10 minutes, put it in a grinder, crush it for 10 minutes, pass it through a 1500 mesh sieve, put it in 50mL of 2.5mol / L sodium hydroxide solution, stir it for 30 minutes, wash and dry it to obtain pretreated shell powder, put the pretreated shell powder in a muffle furnace, calcine it at 900℃ for 2.5h, and then cool it to room temperature to obtain calcined shell powder, add 2.5g of calcined shell powder into 80mL of deionized water, stir evenly, add 3.5g of hexadecyltrimethylammonium bromide, filter it, wash it with deionized water 3 times, and dry it in an oven at 85℃ for 15min to obtain modified calcined shell powder.

[0083] The difference between this comparative example and Example 1 is that hexadecyltrimethylammonium bromide and cerium nitrate hexahydrate are not added, and the remaining steps and raw materials are the same as those of Example 1.

[0084] Wash 5g of shell powder with deionized water for 5 times, put it in a 65℃ forced air drying oven and dry it for 10 minutes, put it in a grinder and crush it for 10 minutes, pass it through a 1500-mesh sieve, put it in 50mL of 2.5mol / L sodium hydroxide solution, stir it for 30 minutes, wash and dry it to obtain pretreated shell powder. Put the pretreated shell powder in a muffle furnace, calcine it at 900℃ for 2.5 hours, and then cool it to room temperature to obtain modified calcined shell powder.

[0085] Example 2 The sand-based composite aerogel is prepared by the following steps:

[0086] B1. Wash 1.8g of sand with deionized water to remove surface impurities, dry in an oven at 70°C, place in 50mL of ethanol, add 5g of glucose and 0.25g of citric acid, stir evenly, add 0.5mL of 36% hydrochloric acid, stir and react at 70°C for 30min, filter, wash and dry, place in a tube furnace, add 5mL of potassium hydroxide, introduce nitrogen, carbonize at 800°C for 3h, cool to room temperature, take out, wash with deionized water until the washing liquid is neutral, and dry in an oven at 70°C for 10min to obtain sand loaded with porous carbon;

[0087] B2. Add 3.5g tocopherol to 20mL ethanol and stir evenly. Add 4.5g sand loaded with porous carbon and place in a sealed container. After adsorption at -0.04MPa, heat at 85°C until the organic solvent evaporates to obtain a solid. Add 0.47g melamine formaldehyde resin and 0.5g cellulose nanofibers to 100mL deionized water and stir at 1500r / min for 5h to make them evenly dispersed. Add 0.2mL 4M hydrochloric acid solution to adjust the pH to 0.1. Add 0.25g methyltrimethoxysilane and 4.5g solid, stir and react for 2h. Freeze-dry at -30°C for 2h to obtain a sand-based composite aerogel.

[0088] The difference between this comparative example and Example 2 is that the sand supporting the porous carbon is replaced by sand, and the remaining steps and raw materials are the same as Example 2.

[0089] The difference between this comparative example and Example 2 is that melamine formaldehyde resin and cellulose nanofibers are not added, and the remaining steps and raw materials are the same as those of Example 2.

[0090] 1.8 g of sand was washed with deionized water, dried in an oven at 70°C, placed in 50 mL of ethanol, 5 g of glucose and 0.25 g of citric acid were added, stirred evenly, 0.5 mL of 36% hydrochloric acid was added, and the mixture was stirred and reacted at 70°C for 30 min. After filtration, washing, and drying, the mixture was placed in a tubular furnace, 5 mL of potassium hydroxide was added for activation, nitrogen was introduced, and the mixture was carbonized at 800°C for 3 h. The mixture was cooled to room temperature, taken out, washed, and dried to obtain sand loaded with porous carbon. 3.5 g of antioxidant was added to 20 mL of ethanol, stirred evenly, 4.5 g of sand loaded with porous carbon was added, and the mixture was placed in a sealed container. After the adsorption was completed at -0.04 MPa, the mixture was heated at 85°C until the organic solvent evaporated to obtain a sand-based composite aerogel.

[0091] Example 3 A flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder comprises the following raw materials in parts by mass: 80 parts of polypropylene, 40 parts of modified calcined shell powder, 41 parts of silica sol, 40 parts of expanded perlite, 10 parts of sand-based composite aerogel, 5 parts of vinyltrimethoxysilane, 2 parts of paraffin, 3 parts of stearic acid, and 0.01 parts of decabromodiphenylethane.

[0092] A preparation process of a flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder, comprising the following steps:

[0093] S1. Add the modified calcined shell powder to silica sol (silica sol is mixed with methyltriethoxysilane, tetraethoxysilane, ethanol and deionized water in a molar ratio of 1:0.3:8:6), stir evenly, add 60% hydrochloric acid to adjust the pH to 2.5, stir for 25 minutes, add 36% ammonia water to adjust the pH to 7, add expanded perlite, evacuate to -0.04MPa, take out after adsorption, place in 20mL ethanol for aging for 30 minutes, and dry to obtain a solid;

[0094] S2. Mix polypropylene, the solid prepared in step S1, sand-based composite aerogel, vinyl trimethoxysilane, paraffin, stearic acid and decabromodiphenylethane, stir, and place in a twin-screw extruder. When the temperature of the first section of the twin-screw extruder is 175°C, the temperature of the second section is 190°C, the temperature of the third section is 215°C, the rotation speed is 140rpm, and the aspect ratio of the twin-screw extruder is 20:1, extrude granulation, place the granules in a mold, press them to form a composite sheet, and then die-cut and print to obtain a polypropylene plastic fresh-keeping box.

[0095] Example 4 A flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder comprises the following raw materials in parts by mass: 90 parts of polypropylene, 50 parts of modified calcined shell powder, 45 parts of silica sol, 45 parts of expanded perlite, 15 parts of sand-based composite aerogel, 8 parts of zirconate coupling agent, 2.5 parts of cyclohexanol, 3.5 parts of dibutyl phthalate, and 0.02 parts of brominated epoxy resin.

[0096] A preparation process of a flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder, comprising the following steps:

[0097] S1. Add the modified calcined shell powder to silica sol (silica sol is mixed with methyltriethoxysilane, tetraethoxysilane, ethanol and deionized water in a molar ratio of 1:0.3:12:8), stir evenly, add 60% hydrochloric acid to adjust the pH to 2.5, stir for 25 minutes, add 36% ammonia water to adjust the pH to 7, add expanded perlite, evacuate to -0.04MPa, take out after adsorption, place in 25mL ethanol for aging for 30 minutes, and dry to obtain a solid;

[0098] S2. Mix polypropylene, the solid prepared in step S1, sand-based composite aerogel, zirconate coupling agent, cyclohexanol, dibutyl phthalate, and brominated epoxy resin, stir, and place in a twin-screw extruder. When the temperature of the first section of the twin-screw extruder is 175°C, the temperature of the second section is 190°C, the temperature of the third section is 215°C, the rotation speed is 140rpm, and the aspect ratio of the twin-screw extruder is 20:1, extrude and granulate, place the granules in a mold, press them to form a composite sheet, and then die-cut and print to obtain a polypropylene plastic fresh-keeping box.

[0099] Example 5 A flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder, comprising the following raw materials in parts by mass: 100 parts of polypropylene, 60 parts of modified calcined shell powder, 49 parts of silica sol, 50 parts of expanded perlite, 20 parts of sand-based composite aerogel, 10 parts of vinyltrimethoxysilane, 3 parts of paraffin, 5 parts of stearic acid, and 0.03 parts of brominated polystyrene.

[0100] A preparation process of a flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder, comprising the following steps:

[0101] S1. Add the modified calcined shell powder to silica sol (silica sol is mixed with methyltriethoxysilane, tetraethoxysilane, ethanol and deionized water in a molar ratio of 1:0.3:16:12), stir evenly, add 60% hydrochloric acid to adjust the pH to 2.5, stir for 25 minutes, add 36% ammonia water to adjust the pH to 7, add expanded perlite, evacuate to -0.04MPa, and after adsorption, place in 30mL ethanol for aging for 30 minutes, and dry in an oven at 70°C for 10 minutes to obtain a solid;

[0102] S2. Mix polypropylene, the solid prepared in step S1, sand-based composite aerogel, vinyltrimethoxysilane, paraffin, stearic acid, and brominated polystyrene, stir, and place in a twin-screw extruder. When the temperature of the first section of the twin-screw extruder is 175°C, the temperature of the second section is 190°C, the temperature of the third section is 215°C, the rotation speed is 140rpm, and the aspect ratio of the twin-screw extruder is 20:1, extrude and granulate, place the granules in a mold, press them to form a composite sheet, and then die-cut and print to obtain a polypropylene plastic fresh-keeping box.

[0103] The difference between this comparative example and Example 4 is that the modified calcined shell powder is replaced by the material prepared in Comparative Example 1, and the remaining steps are synchronized with Example 4.

[0104] The difference between this comparative example and Example 4 is that the modified calcined shell powder is replaced by the material prepared in Comparative Example 2, and the remaining steps are synchronized with Example 4.

[0105] The difference between this comparative example and Example 4 is that the sand-based composite aerogel is replaced by the material prepared in Comparative Example 3, and the remaining steps are synchronized with Example 4.

[0106] The difference between this comparative example and Example 4 is that the sand-based composite aerogel is replaced by the material prepared in Comparative Example 4, and the remaining steps are synchronized with Example 4.

[0107] The performance of the polypropylene plastic fresh-keeping boxes prepared in Examples 3-5 and Comparative Examples 5-8 is now tested;

[0108] Rotten fruit experiment: detect the rotten fruit rate of litchi in each packaging container during 48 hours of transportation. The experimental method is to put fresh litchi in the polypropylene plastic fresh-keeping box prepared above, and open the box and count the average number of rotten fruits after 48 hours of transportation;

[0109] Antibacterial experiment: The time required for the fruit to become moldy when the polypropylene plastic fresh-keeping box prepared above is loaded with perishable fruits is tested. 10 perishable fruits whose surfaces have been wiped with sterile water are placed in the polypropylene plastic fresh-keeping box prepared above for transportation. At 20:00 every day, check whether there are mold spots in the polypropylene plastic fresh-keeping box, and calculate the antibacterial rate.

[0110] The mechanical properties of the polypropylene plastic fresh-keeping box prepared above were tested according to the national standard GB18173.1-2012 "Polymer Waterproof Materials Part 1 Sheet Materials"; the flame retardant properties of the polypropylene plastic fresh-keeping box prepared above were tested according to the national standard GB / T2406.2-2009; the test results are shown in Table 1 below:

[0111] Table 1

[0112]

[0113] It can be seen from the data in Table 1 that in Example 5, no cerium nitrate hexahydrate was added, and the prepared modified calcined shell powder was added to a polypropylene plastic fresh-keeping box, and its preservation performance and thermal stability decreased. This may be because a cerium carbonate layer was formed between the layers of the calcined shell powder, which exhibited good barrier properties and could effectively prevent the penetration of moisture, oxygen and other harmful substances, and the formed nano cerium oxide had high thermal stability; in Example 6, no hexadecyltrimethylammonium bromide and cerium nitrate hexahydrate were added, and the prepared modified calcined shell powder was added to a polypropylene plastic fresh-keeping box, and its preservation performance decreased. This may be because the organic intercalant was intercalated between the layers of the calcined shell powder, expanding the interlayer distance of the shell powder, increasing the adsorption capacity of the shell powder, and more efficiently removing the odor and moisture in the fresh-keeping box, thereby extending the shelf life. The shelf life of food; in Comparative Example 7, the sand loaded with porous carbon is replaced by sand, and the prepared sand-based composite aerogel is added to a polypropylene plastic fresh-keeping box, and its flame retardant and mechanical properties are reduced. This may be because the porous carbon also has excellent fire retardant properties, and the porous carbon has excellent adsorption properties, which can adsorb and fix metal elements such as aluminum and iron in the sand to avoid affecting the performance of the fresh-keeping box; in Comparative Example 8, melamine formaldehyde resin and cellulose nanofibers are not added, and the prepared sand-based composite aerogel is added to a polypropylene plastic fresh-keeping box, and its flame retardant properties are reduced. This may be because the melamine formaldehyde resin exhibits excellent flame retardant properties, and the melamine formaldehyde resin and cellulose nanofibers form aerogel, which improves the stability of sand and antioxidants in the plastic fresh-keeping box and avoids migration and precipitation.

[0114] The data in Table 1 show that the polypropylene plastic fresh-keeping box prepared in Examples 3-5 not only has good fresh-keeping performance and antioxidant performance, but also has good waterproof performance, flame retardant performance and air permeability. The modified calcined shell powder is added to the silica sol, stirred evenly, hydrochloric acid is added, adjusted to 2.5, stirred, 36% ammonia water is added to adjust the pH to 7, and expanded perlite is added. After adsorption, it is taken out, placed in ethanol for aging, and dried to obtain a solid; polypropylene, the solid prepared in step S1, the sand-based composite aerogel, coupling agent, dispersant, plasticizer, and flame retardant are mixed, stirred, placed in a twin-screw extruder, extruded and granulated, the particles are placed in a mold, pressed, and a composite sheet is formed, and then die-cut and printed to obtain a polypropylene plastic fresh-keeping box that meets the test performance requirements, while the polypropylene plastic fresh-keeping box prepared in Comparative Examples 5-8 does not meet the performance requirements, indicating that the polypropylene plastic fresh-keeping box prepared by the present invention not only has good fresh-keeping performance and antioxidant performance, but also has good waterproof performance, flame retardant performance and air permeability.

[0115] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0116] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder, characterized in that: The invention comprises the following raw materials in parts by weight: 80-100 parts of polypropylene, 40-60 parts of modified calcined shell powder, 41-49 parts of silica sol, 40-50 parts of expanded perlite, 10-20 parts of sand-based composite aerogel, 5-10 parts of coupling agent, 2-3 parts of dispersant, 3-5 parts of plasticizer, and 0.01-0.03 parts of flame retardant; The modified calcined shell powder is prepared by calcining the pretreated shell powder at high temperature, mixing it with a cerium source and an organic intercalation agent, and then subjecting it to hydrothermal treatment; The pretreated shell powder is prepared by washing the shell powder, grinding it into powder, sieving it, and treating it with an alkali agent; The sand-based composite aerogel is prepared by mixing porous carbon-loaded sand with an antioxidant, adding the mixture to cellulose nanofibers and melamine formaldehyde resin for cross-linking, and then freeze-drying. The sand-based composite aerogel is specifically prepared by the following steps: The antioxidant was added to ethanol and stirred evenly. The porous carbon-loaded sand was added and placed in a sealed container. After the adsorption was completed at -0.04 MPa, the mixture was heated at 85°C until the organic solvent was volatilized to obtain a solid. The melamine formaldehyde resin and cellulose nanofibers were added to deionized water and stirred at 1500 r / min for 5 h to make them evenly dispersed. 0.2 mL of 4 M hydrochloric acid solution was added to adjust the pH to 0.

1. Methyltrimethoxysilane and the solid were added and stirred for 2 h. The mixture was freeze-dried at -30°C for 2 h to obtain a sand-based composite aerogel. The porous carbon-loaded sand is prepared by washing and drying the sand, mixing it with a carbon precursor and a connecting agent, and then carbonizing it at high temperature.

2. The flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder according to claim 1, characterized in that: The cerium source is selected from cerium nitrate hexahydrate, cerium chloride and cerium sulfate.

3. The flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder according to claim 1, characterized in that: The organic intercalant is selected from any one of tetrabutylammonium bromide, hexadecyltrimethylammonium bromide, dodecyltrimethylammonium bromide and sodium diethylphosphinate.

4. The flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder according to claim 1, characterized in that: The alkali treatment agent is selected from one of sodium hydroxide solution and potassium hydroxide solution; the concentration of the alkali treatment agent is 1.2-3.5 mol / L; the aperture of the sieve mesh is 1000-2000 mesh.

5. The flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder according to claim 1, characterized in that: The antioxidant is selected from any one of tocopherol, butylated hydroxytoluene and ascorbic acid; the cellulose nanofiber has a length of 2-10 μm and a diameter of 10-50 nm.

6. The flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder according to claim 1, characterized in that: The carbon precursor is selected from one of glucose, rice husk powder, starch and bagasse.

7. The flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder according to claim 1, characterized in that: The expanded perlite has a particle size of 0.5-0.8 mm and a pore size of 40-50 μm.

8. The flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder according to claim 1, characterized in that: The flame retardant is selected from any one of decabromodiphenylethane, brominated epoxy resin and brominated polystyrene; and the dispersant is selected from paraffin or cyclohexanol.

9. A process for preparing a flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: S1. Take the formula mass parts of raw materials, add the modified calcined shell powder to the silica sol, stir evenly, add hydrochloric acid to adjust the pH to 2.5, stir, then add ammonia to adjust the pH to 7, add expanded perlite, after adsorption is complete, take out, place in ethanol for aging, and dry to obtain a solid; S2. Mix polypropylene, the solid prepared in step S1, the sand-based composite aerogel, the coupling agent, the dispersant, the plasticizer, and the flame retardant, stir, place in a twin-screw extruder, extrude and granulate, place the granules in a mold, press to form a composite board, and then die-cut and print to obtain a polypropylene plastic fresh-keeping box.

10. The flame-retardant polypropylene plastic fresh-keeping box with added sand and calcined shell powder according to claim 9, characterized in that: The temperature of the first section of the twin-screw extruder is 170-180°C, the temperature of the second section is 185-195°C, and the temperature of the third section is 210-220°C; the rotation speed is 130-150rpm, and the aspect ratio of the twin-screw extruder is 18-22:0.5-1.5.

Citation Information

Patent Citations

  • Method for preparing aquatic product cleaning agent based on shell powder

    CN104877808A

  • Compound thermal insulation material based on fiber and preparation method of compound thermal insulation material

    CN110372257A