A high-performance composite material for pipes and preparation method thereof
By using a combination of long carbon chain semi-aromatic nylon, whiskers, and aramid nanofibers in nylon pipes, the strength and toughness problems of nylon pipes under high pressure and low temperature conditions have been solved, and high-performance composite materials have been prepared and improved. It improves the safety and service life of pipelines and promotes the development of the pipeline industry.
Patent Information
- Application Number
- CN202410837570.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-26
AI Technical Summary
Existing nylon pipes have problems such as low strength, poor toughness, and poor dimensional stability under high pressure and low temperature conditions, making it difficult to meet the needs of use in complex terrain and various load conditions.
Long carbon chain semi-aromatic nylon is used as the matrix resin, combined with whiskers and aramid nanofibers as composite reinforcing fillers, and PA66 is added during melt processing to form a composite material with high strength, high toughness and good fluidity.
It has achieved the preparation of high-performance composite materials with excellent mechanical properties and dimensional stability, can maintain the safety and service life of pipelines under complex conditions, and promotes the industrialization and market competitiveness of the pipeline industry.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, and in particular relates to a composite material for high-performance pipelines and a preparation method thereof. Background Art
[0002] Replacing steel with plastic is the development trend of materials and transportation pipelines in the world, and the research on high-performance and low-cost plastics is the focus of pipeline research. The special properties of composite materials provide broad prospects for the research of high-performance composite plastics.
[0003] Thermoplastic composite pipes have the advantages of good corrosion resistance, light weight, easy installation and transportation, etc., and are widely used in oil and gas field transportation, fire protection pipelines, residential sewage pipe networks and other fields. Most pipelines are laid underground, which can protect the pipelines from the influence of the external environment and increase the service life of the pipelines. However, due to the influence of factors such as topography, increasing transmission pressure, and tensile torsion during installation, the pipeline system may break and be accompanied by the leakage of toxic liquids and gases. The wall of the composite pipe not only has to bear the axial load, but also has to meet the sealing of the fluid in the pipe. The interaction of multiple loads makes the composite pipe wall the most critical and most prone to failure in the entire pipe network system. The quality of the pipe wall directly affects the service life and safety of the pipeline. Therefore, studying the rationality of pipe design and improving the load-bearing performance of the pipe are of great significance to the safe and stable transportation of the pipe network system.
[0004] At present, high-performance plastic pipes are mainly high-density polyethylene and nylon. High-density polyethylene pipes are generally made of double-walled fibers. Although they have the advantages of corrosion resistance, long service life, and a wide range of applications, their manufacturing process is complex and their manufacturing cost is high. Nylon pipes are easy to construct and have high production efficiency. The pipes are high-strength, light, and wear-resistant. They can be used to transport a variety of materials. They are also low-priced and conducive to industrial promotion. However, the existing nylon pipes have low strength, poor toughness, and poor dimensional stability. They are applied to thermal power generation, channel dredging, metallurgy, mining and other industries, and have problems such as low compressive strength and low toughness. Therefore, it is of great theoretical and practical significance to carry out research on the modification of nylon. At present, the modification research on nylon pipes at home and abroad usually adopts the addition of single glass fiber or aramid fiber to improve product performance. Its tensile strength is high, but its toughness is low, and it is difficult to meet the use under low temperature conditions. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a high-performance composite material for pipelines, which has the advantages of high strength and high impact resistance.
[0006] The present invention is achieved through the following technical solutions:
[0007] A high-performance composite material for pipes, comprising the following components in parts by weight:
[0008] 80-100 parts of long carbon chain semi-aromatic nylon, 5-20 parts of PA66, 20-30 parts of whiskers, 5-10 parts of aramid nanofibers, 5-10 parts of flame retardants, 2-6 parts of coupling agents, 1-2 parts of nucleating agents, and 0.1-1 parts of lubricants;
[0009] The whisker has a length of 30-80 μm and a diameter of 1-4 μm; the aramid nanofiber has a length of 30-100 μm and a diameter of 20-80 nm.
[0010] There are many types of polyamides, including aliphatic, semi-aromatic and fully aromatic polyamides, such as PA66, PA6T, PPTA, etc. Although aliphatic polyamides are cheap, they have poor mechanical properties, high water absorption, and unstable dimensions, making it difficult to meet the use requirements of pipeline materials. Short-chain semi-aromatic polyamides have a high melting point, generally close to 400°C. At this temperature, the polymer is easily thermally decomposed, so it cannot be melt-molded, which does not meet the technical requirements of high fluidity for pipe wall manufacturing; at the same time, short-chain semi-aromatic polyamides are not tough enough and are prone to cracking at low temperatures. Although fully aromatic polyamides have high strength, they also have the problems of high processing temperature, low toughness, and poor fluidity, and it is difficult to toughen and modify them by adding inorganic fillers such as fibers. Long-chain semi-aromatic nylons have the advantages of good toughness, high fluidity, and low processing temperature of aliphatic nylons and high mechanical strength of fully aromatic polyamides, and have excellent comprehensive performance of dimensional stability and melt moldability, are resistant to solvent corrosion, have high fatigue strength, and have low shrinkage, which can meet the basic use requirements of composite materials for pipelines.
[0011] In order to further improve the toughness and mechanical strength of long carbon chain semi-aromatic nylon, the present invention uses whiskers and aramid nanofibers as composite reinforcing fillers. Although glass fiber has higher tensile strength, its impact toughness is lower and its length is longer, so it is difficult to be evenly dispersed in long carbon chain semi-aromatic nylon. Whiskers have higher integrity than glass fiber and fewer crystal defects. It combines the advantages of inorganic glass fiber and organic synthetic fiber, and has both the high strength of glass fiber and the high toughness of organic fiber. Single whisker reinforcing filler has poor dispersibility in long carbon chain semi-aromatic nylon, and toughness improvement is limited. Aramid nanofibers have nanostructures, and their length is comparable to whiskers, and they all belong to micron-level lengths, and they can be interlaced with whiskers to form continuous structures, improving the dispersibility of whiskers. And aramid nanofibers and matrix resins all belong to nylon materials, and there is no compatibility problem between the two, which not only saves the addition of compatibilizers, but also improves the dispersibility of inorganic fillers.
[0012] Compared with long carbon chain semi-aromatic nylon, PA66 has lower melting point and higher fluidity. During the melt processing, PA66 melts in advance, which can improve the dispersion of whiskers, aramid nanofibers, flame retardants, coupling agents, nucleating agents, and lubricants, and improve the mechanical properties of composite materials. Attention should be paid to the amount of PA66 added. If the amount of PA66 is too small, it is difficult to play a dispersing role; if the amount is too large, it is easy to reduce the mechanical properties of the composite material.
[0013] Furthermore, the long carbon chain semi-aromatic nylon is at least one of PA9T, PA9I, PA10T, PA10I, PA11T, PA11I, PA12T, PA12I, PA14T, and PA14I; further, the long carbon chain semi-aromatic nylon is a mixture of PA9T and PA12T in a mass ratio of 1:1.
[0014] Furthermore, the whiskers are at least one of calcium carbonate whiskers, zinc oxide whiskers, magnesium sulfate whiskers, and calcium sulfate whiskers.
[0015] Furthermore, the aramid nanofiber is poly(p-phenylene terephthalamide) nanofiber.
[0016] Furthermore, the flame retardant is at least one of aluminum diethylphosphinate, melamine polyphosphate, and melamine cyanurate.
[0017] Furthermore, the coupling agent is at least one of KH550, KH560, and KH570.
[0018] Furthermore, the nucleating agent is at least one of talc, silicon dioxide, magnesium oxide and aluminum oxide.
[0019] Furthermore, the lubricant is at least one of silicone oil, polyethylene wax, calcium stearate, and zinc stearate.
[0020] Furthermore, the PA66 is 10-15 parts.
[0021] The present invention also provides a method for preparing the composite material for high-performance pipelines, comprising the following steps:
[0022] (1) Weigh each component according to the proportion;
[0023] (2) Long carbon chain semi-aromatic nylon, PA66, flame retardant, coupling agent, nucleating agent, and lubricant are added into a twin-screw extruder from a main feed port, and whiskers and aramid nanofibers are added from a side feed port. The product is extruded at an extrusion temperature of 320-340°C and a screw speed of 150-250 r / min.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The present invention uses long carbon chain semi-aromatic nylon as the base resin material, which has the advantages of good toughness and high fluidity of aliphatic nylon and high mechanical strength of aromatic polyamide, and can meet the basic use requirements of composite materials for pipelines. A small amount of PA66 is added, which can be melted in advance during the melt processing, improve the melt fluidity and the dispersion of the filler, and improve the mechanical properties of the composite material.
[0026] 2. The preparation process of the high-performance composite material for pipes of the present invention is consistent with that of conventional reinforced nylon, and has no special requirements for equipment, and no need to improve existing equipment.
[0027] 3. Whiskers and aramid nanofibers, as inorganic and organic composite reinforcing fillers, can interlace to form a continuous structure, improve the interaction between the fibrous filler and the resin, and the composite reinforcing filler is evenly distributed in the nylon resin and has high interfacial bonding performance with the matrix resin, so that the composite material has flexibility while maintaining excellent mechanical strength. It can not only achieve large-scale, non-metallic, lightweight and cheap pipelines, promote the industrial production of the pipeline industry, and improve the market competitiveness of plastic pipelines, but also break through the problem of single performance of traditional pipelines and achieve the unity of strength and toughness, which will help to significantly improve the overall level of my country's pipeline industry. DETAILED DESCRIPTION
[0028] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and carefully in combination with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.
[0029] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0030] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0031] Unless otherwise specified, the component types in Tables 1-3 are consistent, specifically: the whiskers are calcium sulfate whiskers with a length of 50 μm and a diameter of 2 μm; the aramid nanofibers are poly(p-phenylene terephthalamide) nanofibers with a length of 60 μm and a diameter of 60 nm; the flame retardant is a composite flame retardant of diethyl aluminum phosphinate and melamine polyphosphate, and the mass ratio of the two is 1:1; the coupling agent is KH560; the nucleating agent is talc; the lubricant is calcium stearate; the glass fiber has a length of 10 mm and a diameter of 10 μm.
[0032]
[0033]
[0034]
[0035] The preparation method of the composite material for high-performance pipelines in the above-mentioned embodiment and comparative example comprises the following steps:
[0036] (1) Weigh each component according to the proportion;
[0037] (2) Long carbon chain semi-aromatic nylon, PA66, flame retardant, coupling agent, nucleating agent and lubricant are added into a twin-screw extruder from the main feed port, and whiskers and aramid nanofibers (Comparative Examples 1 and 2 do not add whiskers or aramid nanofibers; Comparative Example 5 uses glass fibers instead of whiskers) are added from the side feed port. The product is extruded at an extrusion temperature of 330°C and a screw speed of 200 r / min to obtain a product.
[0038] Performance test: The high-performance composite materials for pipes prepared in the examples and comparative examples were injection molded into standard styles, and mechanical and flame retardant performance tests were performed under the same test conditions. The results are shown in Tables 4-6 below.
[0039]
[0040]
[0041]
[0042] As can be seen from Tables 4-6, the high-performance composite material for pipes prepared by the present invention has higher strength and better impact toughness, and is a fiber-reinforced composite material with excellent comprehensive performance. As can be seen from Examples 7-12, the compounding of PA9T and PA12T can better improve the mechanical properties of the composite material. At the same time, during the melt processing, PA66 melts in advance, which can improve the dispersibility of fillers such as whiskers, aramid nanofibers, and flame retardants, and improve the mechanical properties of the composite material. As can be seen from Comparative Examples 1-5, when the amount of aramid nanofibers is too small, it is not conducive to the improvement of mechanical properties; when the amount is too large, its long fiber-like structure may be too staggered, and even aramid fiber self-agglomeration may occur, which is not conducive to the dispersion of fillers and leads to reduced mechanical properties of the composite material. It can be seen that the whiskers and aramid nanofibers with reasonable proportions in the present invention as inorganic and organic composite reinforcing fillers can be interlaced to form a continuous structure, improve the interaction between the fiber and the resin, and the composite reinforcing filler is evenly distributed in the nylon resin and has high interfacial bonding performance with the matrix resin, so that the composite material has flexibility while maintaining excellent mechanical strength.
[0043] The above description of the embodiments is to facilitate the understanding and application of the present invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the embodiments herein, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.
Claims
1. A high-performance composite material for pipes, It is characterized in that Contains the following components in parts by weight: 80-100 parts of long carbon chain semi-aromatic nylon, 5-20 parts of PA66, 20-30 parts of whiskers, 5-10 parts of aramid nanofibers, 5-10 parts of flame retardants, 2-6 parts of coupling agents, 1-2 parts of nucleating agents, and 0.1-1 parts of lubricants; The whisker has a length of 30-80 μm and a diameter of 1-4 μm; the aramid nanofiber has a length of 30-100 μm and a diameter of 20-80 nm; The long carbon chain semi-aromatic nylon is a mixture of PA9T and PA12T in a mass ratio of 1:
1.
2. A high-performance composite material for pipes as claimed in claim 1, It is characterized in that The whiskers are at least one of calcium carbonate whiskers, zinc oxide whiskers, magnesium sulfate whiskers, and calcium sulfate whiskers.
3. A high-performance composite material for pipes as claimed in claim 1, It is characterized in that The aramid nanofiber is poly(p-phenylene terephthalamide) nanofiber.
4. A high-performance composite material for pipes as claimed in claim 1, It is characterized in that The flame retardant is at least one of aluminum diethylphosphinate, melamine polyphosphate, and melamine cyanurate.
5. A high-performance composite material for pipes as claimed in claim 1, It is characterized in that The coupling agent is at least one of KH550, KH560 and KH570.
6. A high-performance composite material for pipes as claimed in claim 1, It is characterized in that The nucleating agent is at least one of talc, silicon dioxide, magnesium oxide and aluminum oxide.
7. A high-performance composite material for pipes as claimed in claim 1, It is characterized in that The lubricant is at least one of silicone oil, polyethylene wax, calcium stearate and zinc stearate.
8. The high-performance composite material for pipes according to claim 1, It is characterized in that The PA66 is 10-15 parts.
9. A method for preparing a high-performance composite material for pipes according to any one of claims 1 to 8, It is characterized in that The steps include: (1) Weigh each component according to the proportion; (2) Long carbon chain semi-aromatic nylon, PA66, flame retardant, coupling agent, nucleating agent, and lubricant are added into a twin-screw extruder from a main feed port, and whiskers and aramid nanofibers are added from a side feed port. The product is extruded at an extrusion temperature of 320-340°C and a screw speed of 150-250 r / min.