A method for preparing dark heat-insulating coating using modified carbon black as pigment

Through the combination of modified carbon black, modified starch and highly weather-resistant silicone-acrylic emulsion, a dark-colored thermal insulation coating is prepared, which solves the problem of light pollution of light-colored coatings, achieves efficient thermal insulation and improved spraying performance, and is suitable for building insulation. Thermal applications.

CN118480292BActive Publication Date: 2024-10-01青州市博奥炭黑有限责任公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410930839.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-01
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

When existing light-colored coatings are used for heat insulation, they cause light pollution by reflecting sunlight, affecting traffic safety, and are subject to national restrictions. Dark-colored heat-insulating coatings need to be developed to replace them.

Method used

Using materials such as modified carbon black, modified starch and highly weather-resistant silicone-acrylic emulsion, dark-colored heat-insulating coatings are prepared through stirring and emulsification processes. Using the red and blue phase characteristics of carbon black, polylactic acid coats the carbon black particles and combines them with mica powder. and kaolin and other materials to prepare coatings with deep color and good heat insulation effect.

Benefits of technology

The dark heat-insulating paint prepared is not only deep in color, but also has a heat-insulating effect better than industry standards. It also avoids reflected light pollution, improves spraying efficiency, and meets the high-temperature resistance requirements of building shells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the technical field of coatings, and discloses a method for preparing a dark heat-insulating coating by using modified carbon black as a pigment. 5 to 15 parts of water, 6 to 10 parts of modified starch, 5 to 8 parts of modified carbon black, and 15 to 25 parts of silicone-acrylic emulsion weighed by weight are put into a container and stirred evenly at a speed of 800 to 1200 rpm, and then 10 to 20 parts of water, 6 to 8 parts of carboxymethyl cellulose, 25 to 35 parts of mica powder, 30 to 40 parts of kaolin, 1 to 2 parts of alcohol ester twelve, 0.3 to 0.6 parts of polyether defoamer, and 0.1 to 0.3 parts of isothiazolinone preservative are added and stirred continuously, and stirring is continued at a speed of 800 to 1200 rpm for 30 to 90 minutes to obtain a dark heat-insulating coating. The coating prepared by the invention has a dark color, a good heat-insulating effect, and can effectively prevent reflected light pollution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to a method for preparing a dark-colored heat-insulating coating by using modified carbon black as a pigment. Background Art

[0002] At present, the global temperature is constantly rising, and there are more and more high-temperature days. The requirements for the high-temperature resistance of building shells and equipment used under high temperatures are getting higher and higher. The requirements for the heat insulation of building shells and outdoor equipment are also getting higher and higher. Existing insulation materials usually use light-colored coatings to reflect light to achieve the effect of heat insulation. In order to achieve the maximum reflection effect, the color of the coating will be very light, or even white. However, white or light-colored coatings often reflect a large amount of sunlight and cause visual interference, causing light pollution, and are prone to reflective hazards that endanger traffic safety due to glare; therefore, many countries have established reflective standards for the reflectivity of coatings and restricted the production and use of light-colored coatings, which highlights the importance of developing dark-colored coatings. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a method for preparing a dark heat-insulating coating by using modified carbon black as a pigment. The coating prepared by the method has a dark color and a good heat-insulating effect and can effectively prevent reflected light pollution.

[0004] In order to solve the above technical problems, the technical solution of the present invention is:

[0005] A method for preparing a dark heat-insulating coating by using modified carbon black as a pigment comprises the following steps:

[0006] First, 5 to 15 parts of water, 6 to 10 parts of modified starch, 5 to 8 parts of modified carbon black, and 15 to 25 parts of silicone-acrylic emulsion weighed by weight are put into a container and stirred evenly at a speed of 800 to 1200 rpm, and then 10 to 20 parts of water, 6 to 8 parts of carboxymethyl cellulose, 25 to 35 parts of mica powder, 30 to 40 parts of kaolin, 1 to 2 parts of alcohol ester dodecahydrate, 0.3 to 0.6 parts of polyether defoamer and 0.1 to 0.3 parts of isothiazolinone preservative weighed by weight are added and stirred continuously, and stirring is continued at a speed of 800 to 1200 rpm for 30 to 90 minutes to obtain a dark heat-insulating coating;

[0007] The preparation method of modified carbon black is as follows: 200g carbon black and 100g silane coupling agent KH560 are added to an alcohol aqueous solution (a mixture of 6kg ethanol and 600g deionized water), and then 20g ammonia water is added dropwise, and after ultrasonic treatment for 15min, the mixture is transferred to a three-necked flask, and stirred at 40°C at a speed of 400r / min for 12 hours. Finally, the obtained product is centrifuged and washed with alcohol for multiple times, and then vacuum dried at 40°C; the above product is placed in a reactor filled with nitrogen, 10kg tetrahydrofuran solution is added, and ultrasonic treatment is performed for 30min, and then 150g polylactic acid is added, and 8g catalyst stannous octoate is added dropwise, and the mixture is condensed and refluxed at a temperature of 50°C for 4h, and after the reaction is completed, the mixture is centrifuged at a speed of 4000r / min for 30min, and after multiple washings with chloroform, the mixture is placed in a drying oven for drying to obtain modified carbon black, and the particle diameter thereof is 200-500nm;

[0008] The preparation method of modified starch is as follows: 500g corn starch is added into water to prepare a solution with a mass concentration of 40%, and stirred at room temperature for 30 minutes to obtain a starch solution; a sodium hypochlorite solution accounting for 3% of the dry weight of starch is added into the starch solution, and a 10% mass concentration hydrochloric acid solution is used to adjust the pH value to 6, and the reaction is maintained at room temperature for 2 hours; after the reaction is completed, the pH value is adjusted to 3.5 with 10% mass concentration hydrochloric acid, and 3% hydrogen peroxide accounting for the dry weight of starch is added to terminate the reaction; after the reaction is completed, the solution is filtered by suction, washed with water 3 times, and the obtained starch filter cake is dried to obtain the finished modified starch.

[0009] Preferably, the dark thermal insulation coating is composed of the following components in proportion by weight: 25 parts of water, 8 parts of modified starch, 6.5 parts of modified carbon black, 20 parts of silicone acrylic emulsion, 7 parts of carboxymethyl cellulose, 30 parts of mica powder, 35 parts of kaolin, 1.5 parts of alcohol ester dodecahydrate, 0.45 parts of polyether defoamer and 0.2 parts of isothiazolinone preservative.

[0010] Preferably, the silicone-acrylic emulsion is a highly weather-resistant silicone-acrylic emulsion, and the preparation method thereof is as follows:

[0011] a. Add a certain amount of 4,4' diphenylmethane diisocyanate ( MDI ), slowly drop an equal amount of hydroxyethyl methacrylate at 40°C, react under nitrogen protection, monitor the reaction progress with the di-n-butylamine method until it approaches the theoretical value, and slowly drop a quantitative PEG400 ( MDI and PEG400 in an equal molar ratio), heat-retaining reaction until the reaction is complete, and then distilling under reduced pressure for purification, thus obtaining a polyurethane macromonomer terminated with a double bond;

[0012] b. 800kg of deionized water was added to the reactor, stirred at 40rpm, and 7kg of sodium lauryl polyoxyethylene ether sulfate, 0.5kg of sodium phosphate, 7kg of sodium 2-acrylamido-2-methylpropane sulfonate (COPS-1) and 2kg of sodium bicarbonate were added successively, and stirred for 15min to dissolve and mix evenly to obtain a kettle liquid;

[0013] c. Add 500kg of deionized water to the emulsifying kettle, start stirring at 50rpm, add 10kg of 3-allyloxy-2-hydroxypropanesulfonate (COPS-2), 0.5kg of n-pentanol, stir for 15min, add 500kg of polyurethane macromonomer, 350kg of styrene, 250kg of butyl acrylate, 20kg of acrylic acid, 13kg of acrylamide, stir for 30min to obtain a monomer emulsion, and take out 200kg as a seed monomer emulsion, add the remaining 3kg of sodium persulfate (pre-dissolved in 30kg of water), and continue stirring for 15min to obtain a core monomer emulsion;

[0014] d. 0.7 kg of sodium persulfate was dissolved in 10 kg of water to obtain a seed initiator solution;

[0015] e. 0.4 kg of sodium persulfate was dissolved in 10 kg of water to obtain a shell initiator solution;

[0016] f. Heat the reactor liquid to 75°C, pass nitrogen for 5 minutes and then remove the nitrogen, then add the seed monomer emulsion, add the seed initiator solution after 3 minutes, continue to heat to 80°C, and keep warm for 30 minutes;

[0017] g. After the insulation is completed, the core monomer emulsion is added dropwise to the reactor using a metering pump for 3 hours; after the addition is completed, 200 kg of acrylic acid is added, and after 5 minutes, the shell initiator solution is added and the temperature is kept for 1 hour;

[0018] h. Add 50kg vinyl triisopropylsilane, 100kg γ-methacryloxypropyl triethoxysilane, dissolve 0.5kg sodium hydroxide in 10kg deionized water, add to the reactor, stir for 20min to 30min, keep the temperature at 75℃ to 80℃, and keep warm for 1h to 2h;

[0019] i. Cool the reactor to 50°C, add 33.3% mass concentration of ammonia dilution (10kg ammonia diluted with 30kg water), then add 10% mass concentration of fungicide dilution (3kg BM6 diluted with 30kg water), stir for 30 minutes; filter the material with a 200-mesh filter to obtain a highly weather-resistant silicone acrylic emulsion.

[0020] Preferably, the polyether defoamer is a GPES defoamer.

[0021] Due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0022] The invention utilizes the characteristics of the red phase and the blue phase of carbon black, and prepares carbon black particles wrapped with polylactic acid with a particle diameter of 200-500nm by modifying the carbon black, and then mixes the carbon black particles with modified starch, high weather-resistant silicone acrylic emulsion and thermal insulation material to prepare a dark thermal insulation coating. The adhesion, thermal insulation and antifouling properties of the coating all meet or exceed the industry standards. The specially prepared modified starch has good fluidity, high transparency, good film-forming property, anti-coagulation, and certain emulsification, and can be used as a thickener and film-forming agent, so that the coating can be directly sprayed onto the surface of the building without using a primer, thereby improving the spraying efficiency.

[0023] In conclusion, the coating of the present invention has a dark color, good heat insulation effect, and can effectively prevent reflected light pollution. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is further described below in conjunction with embodiments:

[0025] Example 1: Preparation of modified carbon black

[0026] 200g carbon black and 100g silane coupling agent KH560 are added to an alcohol aqueous solution (a mixture of 6kg ethanol and 600g deionized water), and then 20g ammonia water is added dropwise. After ultrasonic treatment for 15min, the mixture is transferred to a three-necked flask and stirred at 40°C at a speed of 400r / min for 12 hours. Finally, the obtained product is centrifuged and washed with alcohol for multiple times and then vacuum dried at 40°C. The above product is placed in a reactor filled with nitrogen, 10kg tetrahydrofuran solution is added, and ultrasonic treatment is performed for 30min. Then 150g polylactic acid is added, and 8g catalyst stannous octoate is added dropwise. The mixture is condensed and refluxed at a temperature of 50°C for 4h. After the reaction is completed, the mixture is centrifuged at a speed of 4000r / min for 30min, washed with chloroform for multiple times, and then dried in a drying oven to obtain modified carbon black with a particle diameter of 200-500nm.

[0027] Example 2: Preparation of modified starch

[0028] 500g corn starch was added into water to prepare a solution with a mass concentration of 40%, and stirred at room temperature for 30 minutes to obtain a starch solution; a sodium hypochlorite solution (10% mass concentration sodium hypochlorite solution) accounting for 3% of the dry weight of starch was added into the starch solution, and a 10% mass concentration hydrochloric acid solution was used to adjust the pH value to 6, and the reaction was maintained at room temperature for 2 hours; after the reaction, the pH value was adjusted to 3.5 with a 10% mass concentration hydrochloric acid, and 3% hydrogen peroxide accounting for the dry weight of starch was added to terminate the reaction; after the reaction, suction filtration was performed, and the starch cake was washed with water 3 times, and the finished modified starch was obtained by drying.

[0029] Example 3: Preparation of High Weathering Resistant Silicone Acrylic Emulsion

[0030] a. Add a certain amount of 4,4' diphenylmethane diisocyanate ( MDI ), slowly drop an equal amount of hydroxyethyl methacrylate at 40°C, react under nitrogen protection, monitor the reaction progress with the di-n-butylamine method until it approaches the theoretical value, and slowly drop a quantitative PEG400 ( MDI and PEG400 in an equal molar ratio), heat-retaining reaction until the reaction is complete, and then distilling under reduced pressure for purification, thus obtaining a polyurethane macromonomer terminated with a double bond;

[0031] b. 800kg of deionized water was added to the reactor, stirred at 40rpm, and 7kg of sodium lauryl polyoxyethylene ether sulfate, 0.5kg of sodium phosphate, 7kg of sodium 2-acrylamido-2-methylpropane sulfonate (COPS-1) and 2kg of sodium bicarbonate were added successively, and stirred for 15min to dissolve and mix evenly to obtain a kettle liquid;

[0032] c. Add 500kg of deionized water to the emulsifying kettle, start stirring at 50rpm, add 10kg of 3-allyloxy-2-hydroxypropanesulfonate (COPS-2), 0.5kg of n-pentanol, stir for 15min, add 500kg of polyurethane macromonomer, 350kg of styrene, 250kg of butyl acrylate, 20kg of acrylic acid, 13kg of acrylamide, stir for 30min to obtain a monomer emulsion, and take out 200kg as a seed monomer emulsion, add the remaining 3kg of sodium persulfate (pre-dissolved in 30kg of water), and continue stirring for 15min to obtain a core monomer emulsion;

[0033] d. 0.7 kg of sodium persulfate was dissolved in 10 kg of water to obtain a seed initiator solution;

[0034] e. 0.4 kg of sodium persulfate was dissolved in 10 kg of water to obtain a shell initiator solution;

[0035] f. Heat the reactor liquid to 75°C, pass nitrogen for 5 minutes and then remove the nitrogen, then add the seed monomer emulsion, add the seed initiator solution after 3 minutes, continue to heat to 80°C, and keep warm for 30 minutes;

[0036] g. After the insulation is completed, the core monomer emulsion is added dropwise to the reactor using a metering pump for 3 hours; after the addition is completed, 200 kg of acrylic acid is added, and after 5 minutes, the shell initiator solution is added and the temperature is kept for 1 hour;

[0037] h. Add 50kg vinyl triisopropylsilane, 100kg γ-methacryloxypropyl triethoxysilane, dissolve 0.5kg sodium hydroxide in 10kg deionized water, add to the reactor, stir for 20min to 30min, keep the temperature at 75℃ to 80℃, and keep warm for 1h to 2h;

[0038] i. Cool the reactor to 50°C, add 33.3% mass concentration of ammonia dilution (10kg ammonia diluted with 30kg water), then add 10% mass concentration of fungicide dilution (3kg BM6 diluted with 30kg water), stir for 30 minutes; filter the material with a 200-mesh filter to obtain a highly weather-resistant silicone acrylic emulsion.

[0039] Example 4: Dark thermal insulation coating 1

[0040] First, 5 parts of water, 6 parts of modified starch, 5 parts of modified carbon black, and 15 parts of silicone-acrylic emulsion weighed by weight were put into a container with a stirring device and stirred at 1200rpm, and then 10 parts of water, 6 parts of carboxymethyl cellulose, 25 parts of mica powder, 30 parts of kaolin, 1 part of alcohol ester twelve, 0.3 parts of GPES type defoamer (polyether defoamer) and 0.1 parts of isothiazolinone preservative were added and continued to stir at 1200rpm for 30min to obtain a dark thermal insulation coating;

[0041] The preparation method of modified starch is as follows: 500g corn starch is added to water to prepare a solution with a mass concentration of 40%, and stirred at room temperature for 30 minutes to obtain a starch solution; a sodium hypochlorite solution (10% mass concentration sodium hypochlorite solution) accounting for 3% of the dry weight of starch is added to the starch solution, and a 10% mass concentration hydrochloric acid solution is used to adjust the pH value to 6, and the reaction is maintained at room temperature for 2 hours; after the reaction is completed, the pH value is adjusted to 3.5 with 10% mass concentration hydrochloric acid, and then 3% hydrogen peroxide accounting for the dry weight of starch is added to terminate the reaction; after the reaction is completed, the mixture is filtered and washed with water 3 times, and the obtained starch filter cake is dried to obtain the finished modified starch;

[0042] The preparation method of modified carbon black is as follows: 200g carbon black and 100g silane coupling agent KH560 are added to an alcohol aqueous solution (a mixture of 6kg ethanol and 600g deionized water), and then 20g ammonia water is added dropwise, and after ultrasonic treatment for 15min, the mixture is transferred to a three-necked flask, and stirred at 40°C at a speed of 400r / min for 12 hours. Finally, the obtained product is centrifuged and washed with alcohol for multiple times, and then vacuum dried at 40°C; the above product is placed in a reactor filled with nitrogen, 10kg tetrahydrofuran solution is added, and ultrasonic treatment is performed for 30min, and then 150g polylactic acid is added, and 8g catalyst stannous octoate is added dropwise, and the mixture is condensed and refluxed at a temperature of 50°C for 4h, and after the reaction is completed, the mixture is centrifuged at a speed of 4000r / min for 30min, and after multiple washings with chloroform, the mixture is placed in a drying oven for drying to obtain modified carbon black, and the particle diameter thereof is 200-500nm;

[0043] The preparation method of silicone acrylic emulsion is as follows: a. In a four-necked flask equipped with a stirrer, a thermometer, and a reflux condenser, add a certain amount of 4,4' diphenylmethane diisocyanate ( MDI ), slowly drop an equal amount of hydroxyethyl methacrylate at 40°C, react under nitrogen protection, monitor the reaction progress with the di-n-butylamine method until it approaches the theoretical value, and slowly drop a quantitative PEG400 ( MDI and PEG400 in an equal molar ratio), heat-retaining reaction until the reaction is complete, and then distilling under reduced pressure for purification, thus obtaining a polyurethane macromonomer terminated with a double bond;

[0044] b. 800kg of deionized water was added to the reactor, stirred at 40rpm, and 7kg of sodium lauryl polyoxyethylene ether sulfate, 0.5kg of sodium phosphate, 7kg of sodium 2-acrylamido-2-methylpropane sulfonate (COPS-1) and 2kg of sodium bicarbonate were added successively, and stirred for 15min to dissolve and mix evenly to obtain a kettle liquid;

[0045] c. Add 500kg of deionized water to the emulsifying kettle, start stirring at 50rpm, add 10kg of 3-allyloxy-2-hydroxypropanesulfonate (COPS-2), 0.5kg of n-pentanol, stir for 15min, add 500kg of polyurethane macromonomer, 350kg of styrene, 250kg of butyl acrylate, 20kg of acrylic acid, 13kg of acrylamide, stir for 30min to obtain a monomer emulsion, and take out 200kg as a seed monomer emulsion, add the remaining 3kg of sodium persulfate (pre-dissolved in 30kg of water), and continue stirring for 15min to obtain a core monomer emulsion;

[0046] d. 0.7 kg of sodium persulfate was dissolved in 10 kg of water to obtain a seed initiator solution;

[0047] e. 0.4 kg of sodium persulfate was dissolved in 10 kg of water to obtain a shell initiator solution;

[0048] f. Heat the reactor liquid to 75°C, pass nitrogen for 5 minutes and then remove the nitrogen, then add the seed monomer emulsion, add the seed initiator solution after 3 minutes, continue to heat to 80°C, and keep warm for 30 minutes;

[0049] g. After the insulation is completed, the core monomer emulsion is added dropwise to the reactor using a metering pump for 3 hours; after the addition is completed, 200 kg of acrylic acid is added, and after 5 minutes, the shell initiator solution is added and the temperature is kept for 1 hour;

[0050] h. Add 50kg vinyl triisopropylsilane, 100kg γ-methacryloxypropyl triethoxysilane, dissolve 0.5kg sodium hydroxide in 10kg deionized water, add to the reactor, stir for 20min to 30min, keep the temperature at 75℃ to 80℃, and keep warm for 1h to 2h;

[0051] i. Cool the reactor to 50°C, add 33.3% mass concentration of ammonia dilution (10kg ammonia diluted with 30kg water), then add 10% mass concentration of fungicide dilution (3kg BM6 diluted with 30kg water), stir for 30 minutes; filter the material with a 200-mesh filter to obtain a highly weather-resistant silicone acrylic emulsion.

[0052] Example 5: Dark Heat Insulation Coating II

[0053] First, 15 parts of water, 10 parts of modified starch, 8 parts of modified carbon black, and 25 parts of silicone-acrylic emulsion weighed by weight are put into a container with a stirring device and stirred at 1200 rpm, and then 20 parts of water, 8 parts of carboxymethyl cellulose, 35 parts of mica powder, 40 parts of kaolin, 2 parts of alcohol ester dodecahydrate, 0.6 parts of GPES defoamer and 0.3 parts of isothiazolinone preservative weighed by weight are added and continued to stir, and stirring is continued at 800 rpm for 90 minutes to obtain a dark thermal insulation coating product;

[0054] The preparation methods of modified starch, modified carbon black and silicone-acrylic emulsion are the same as those in Example 4.

[0055] Example 6: Dark thermal insulation coating three

[0056] First, 10 parts of water, 8 parts of modified starch, 6.5 parts of modified carbon black, and 20 parts of silicone-acrylic emulsion weighed by weight are put into a container with a stirring device and stirred evenly, and then 15 parts of water, 7 parts of carboxymethyl cellulose, 30 parts of mica powder, 35 parts of kaolin, 1.5 parts of alcohol ester dodecahydrate, 0.45 parts of GPES defoamer and 0.2 parts of isothiazolinone preservative weighed by weight are added and stirred continuously, and stirring is continued at 1000rpm for 60min to obtain a dark thermal insulation coating product;

[0057] The preparation methods of modified starch, modified carbon black and silicone-acrylic emulsion are the same as those in Example 4.

[0058] Example 7: Dark Heat Insulation Coating Four

[0059] First, 10 parts of water, 10 parts of modified starch, 5 parts of modified carbon black, and 25 parts of silicone-acrylic emulsion weighed by weight are put into a container with a stirring device and stirred evenly, and then 15 parts of water, 8 parts of carboxymethyl cellulose, 30 parts of mica powder, 30 parts of kaolin, 1 part of alcohol ester twelve, 0.3 parts of GPES defoamer and 0.1 parts of isothiazolinone preservative weighed by weight are added and stirred continuously, and stirring is continued at 1000rpm for 60min to obtain a dark thermal insulation coating product;

[0060] The preparation methods of modified starch, modified carbon black and silicone-acrylic emulsion are the same as those in Example 4.

[0061] Comparative Example 1:

[0062] Unmodified carbon black was used, and carbon black N330 with a particle size of 200 to 500 nm was selected to replace the modified carbon black in Example 6. The other components, weight proportions, and preparation process were the same.

[0063] Comparative Example 2:

[0064] Unmodified common corn starch was used to replace the modified starch in Example 6, and the other components, weight proportions and preparation process were the same.

[0065] Comparative Example 3:

[0066] The PD-6 silicone acrylic emulsion produced by Shandong Baoda New Materials Co., Ltd. was used to replace the silicone acrylic emulsion in Example 6, and the other components, weight portions and preparation process were the same.

[0067] Comparative Example 4:

[0068] Unmodified carbon black is used, and carbon black N330 with a particle size of 200 to 500 nm is selected to replace the modified carbon black in Example 6; unmodified ordinary corn starch is used to replace the modified starch in Example 6; other components, weight portions, and preparation processes are the same.

[0069] Comparative Example 5:

[0070] Unmodified carbon black is used, and carbon black N330 with a particle size of 200 to 500 nm is selected to replace the modified carbon black in Example 6; PD-6 silicone acrylic emulsion produced by Shandong Baoda New Materials Co., Ltd. is used to replace the silicone acrylic emulsion in Example 6; other components, weight portions, and preparation processes are the same.

[0071] Comparative Example 6:

[0072] Unmodified ordinary corn starch is used to replace the modified starch in Example 6; PD-6 silicone acrylic emulsion produced by Shandong Baoda New Materials Co., Ltd. is used to replace the silicone acrylic emulsion in Example 6; other components, weight portions and preparation processes are the same.

[0073] Comparative Example 7:

[0074] Unmodified carbon black is used, and carbon black N330 with a particle size of 200 to 500 nm is selected to replace the modified carbon black in Example 6; unmodified ordinary corn starch is used to replace the modified starch in Example 6; PD-6 silicone acrylic emulsion of Shandong Baoda New Materials Co., Ltd. is used to replace the silicone acrylic emulsion in Example 6; other components, weight portions and preparation processes are the same.

[0075] Product Testing:

[0076] 1. Solar reflectivity and reflection index experiment: The products obtained in Examples 4 to 7 and Comparative Examples 1 to 7 were sprayed to prepare 2 mm thick coatings, and the solar reflectivity (TSR value) and solar reflection index (SRI value) were tested using ASTM E903 and ASTM E1980 standards. The measured data are shown in Table 1.

[0077] 2. Experiment on thermal insulation performance: Temperature sensors were placed on both sides of the 2 mm thick coatings prepared from the products of Examples 4 to 7 and Comparative Examples 1 to 7, and the temperatures of the exposed surface and the unexposed surface were measured to be 500°C, as shown in Table 1.

[0078] 3. Simulated building experiment: The surface of an empty wooden box with a length, width and height of 2 meters was sprayed with 2 mm thick products of Examples 4 to 7 and Comparative Examples 1 to 7 and placed in the sun for six hours. The temperature difference inside and outside the box was measured. The results are shown in Table 1.

[0079]

[0080] Result analysis:

[0081] By testing the products of Examples 4 to 7 and Comparative Examples 1 to 7,

[0082] 1. It can be seen from the solar reflectivity and reflectivity index experimental data that although the solar reflectivity (TSR value) and solar reflectivity index (SRI value) of the products of Examples 4 to 7 of the present invention are much lower than those of white, they are comparable to the solar reflectivity index (40 to 60) of ordinary metal materials, and are significantly improved compared to the TSR value and SRI value of products prepared using ordinary carbon black. This can theoretically prove that the surface material prepared by the present invention has a higher ability to maintain low temperatures.

[0083] 2. From the experimental data on thermal insulation performance, it can be seen that the thermal insulation performance of modified carbon black products is good, which is significantly different from that of unmodified carbon black products.

[0084] 3. Through the thermal insulation experiment of simulated buildings, it can be seen that the actual thermal insulation effect of using modified carbon black products is significantly different from that of using unmodified carbon black products.

[0085] It can be seen that the modified carbon black, modified starch and high weather-resistant silicone-acrylic emulsion of the present application can only be combined together to form a product with the best efficacy. Changing any one of the components will have a negative impact on the product quality and efficacy, among which the modified carbon black has the greatest impact.

[0086] The dark-colored heat-insulating coating prepared by using the components of the present application can be applied to the construction field, has a good heat-insulating effect, and can effectively prevent reflected light pollution.

[0087] It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope limited by the appended claims of the application.

Claims

1. A method for preparing a dark thermal insulation coating using modified carbon black as a pigment, characterized in that: The following steps are involved: First, 5 to 15 parts of water, 6 to 10 parts of modified starch, 5 to 8 parts of modified carbon black, and 15 to 25 parts of silicone-acrylic emulsion weighed by weight are put into a container and stirred evenly at a speed of 800 to 1200 rpm, and then 10 to 20 parts of water, 6 to 8 parts of carboxymethyl cellulose, 25 to 35 parts of mica powder, 30 to 40 parts of kaolin, 1 to 2 parts of alcohol ester dodecahydrate, 0.3 to 0.6 parts of polyether defoamer and 0.1 to 0.3 parts of isothiazolinone preservative weighed by weight are added and stirred continuously, and stirring is continued at a speed of 800 to 1200 rpm for 30 to 90 minutes to obtain a dark heat-insulating coating; The preparation method of modified carbon black is as follows: 200g carbon black and 100g silane coupling agent KH560 are added to an alcohol-water solution, mixed, and then 20g ammonia water is added dropwise, and the mixture is transferred to a three-necked flask after ultrasonic treatment for 15min, and stirred at 40°C at a speed of 400r / min for 12 hours, and finally the obtained product is centrifuged and washed with alcohol for multiple times and then vacuum dried at 40°C; the above product is placed in a reactor filled with nitrogen, 10kg tetrahydrofuran solution is added, ultrasonic treatment is performed for 30min, and then 150g polylactic acid is added, and 8g catalyst stannous octoate is added dropwise, condensed and refluxed at 50°C for 4h, and the reaction is carried out at a speed of 4000r / min for 30min after the reaction is completed, and the modified carbon black is dried in a drying oven after multiple washings with chloroform, and the particle diameter thereof is 200-500nm; The preparation method of modified starch is as follows: 500g corn starch is added into water to prepare a solution with a mass concentration of 40%, and stirred at room temperature for 30 minutes to obtain a starch solution; a sodium hypochlorite solution accounting for 3% of the dry weight of starch is added into the starch solution, and a 10% mass concentration hydrochloric acid solution is used to adjust the pH value to 6, and the reaction is maintained at room temperature for 2 hours; after the reaction is completed, the pH value is adjusted to 3.5 with 10% mass concentration hydrochloric acid, and then 3% hydrogen peroxide accounting for the dry weight of starch is added to terminate the reaction; after the reaction is completed, the solution is filtered by suction, washed with water 3 times, and the obtained starch filter cake is dried to obtain the finished modified starch; The silicone-acrylic emulsion is a highly weather-resistant silicone-acrylic emulsion, and its preparation method is as follows: a. Add a certain amount of 4,4'-diphenylmethane diisocyanate to a four-necked flask equipped with a stirrer, a thermometer, and a reflux condenser, slowly drop an equal amount of hydroxyethyl methacrylate at 40°C, react under nitrogen protection, slowly drop PEG400 with the same molar number as 4,4'-diphenylmethane diisocyanate, keep warm until the reaction is complete, and then purify by vacuum distillation to obtain a polyurethane macromonomer terminated with a double bond; b. 800kg of deionized water was added to the reactor, stirring at a rate of 40rpm, 7kg of sodium lauryl polyoxyethylene ether sulfate, 0.5kg of sodium phosphate, 7kg of sodium 2-acrylamido-2-methylpropane sulfonate and 2kg of sodium bicarbonate were added, stirred for 15min to dissolve and mix evenly to obtain a kettle liquid; c. Add 500kg of deionized water to the emulsifying kettle, start stirring at a rate of 50rpm, add 10kg of 3-allyloxy-2-hydroxypropanesulfonic acid sodium, 0.5kg of n-pentanol, stir for 15min, add 500kg of polyurethane macromonomer, 350kg of styrene, 250kg of butyl acrylate, 20kg of acrylic acid, 13kg of acrylamide, stir for 30min to obtain a monomer emulsion, and take out 200kg as a seed monomer emulsion, add the remaining 3kg of sodium persulfate, and continue stirring for 15min to obtain a core monomer emulsion; d. 0.7 kg of sodium persulfate was dissolved in 10 kg of water to obtain a seed initiator solution; e. 0.4 kg of sodium persulfate was dissolved in 10 kg of water to obtain a shell initiator solution; f. Heat the reactor liquid to 75°C, pass nitrogen for 5 minutes and then remove the nitrogen, then add the seed monomer emulsion, add the seed initiator solution after 3 minutes, continue to heat to 80°C, and keep warm for 30 minutes; g. After the insulation is completed, the core monomer emulsion is added dropwise to the reactor using a metering pump for 3 hours; after the addition is completed, 200 kg of acrylic acid is added, and after 5 minutes, the shell initiator solution is added and the temperature is kept for 1 hour; h. Add 50kg vinyl triisopropylsilane, 100kg γ-methacryloxypropyl triethoxysilane, dissolve 0.5kg sodium hydroxide in 10kg deionized water, add to the reactor, stir for 20min to 30min, keep the temperature at 75℃ to 80℃, and keep warm for 1h to 2h; i. Cool the reactor to 50°C, add 33.3% mass concentration of ammonia diluent, then add 10% mass concentration of fungicide diluent, stir for 30 minutes; filter the material with a 200-mesh filter to obtain a highly weather-resistant silicone-acrylic emulsion.

2. The method for preparing a dark thermal insulation coating using modified carbon black as a pigment according to claim 1, characterized in that: The dark heat-insulating coating is composed of the following components in proportion by weight: 25 parts of water, 8 parts of modified starch, 6.5 parts of modified carbon black, 20 parts of silicone-acrylic emulsion, 7 parts of carboxymethyl cellulose, 30 parts of mica powder, 35 parts of kaolin, 1.5 parts of alcohol ester dodecanone, 0.45 parts of polyether defoaming agent and 0.2 parts of isothiazolinone preservative.

3. The method for preparing a dark thermal insulation coating using modified carbon black as a pigment according to claim 1, characterized in that: The polyether defoamer is a GPES defoamer.

Citation Information

Patent Citations

  • Preparation method of polylactic acid fiber pre-spinning colorant

    CN108084412A

  • Environment-friendly micro-repair asphalt separant and preparation method thereof

    CN114507476A

  • Carbon black slurry for shading fabric as well as preparation method and application of carbon black slurry

    CN115182172A

  • High-weather-resistance silicone-acrylic emulsion for outer wall and production process of high-weather-resistance silicone-acrylic emulsion

    CN116253843A

  • Clarity improver for glossy coloring coating

    JP2015059194A