A kind of impact-resistant and wear-resistant powder coating and preparation method thereof
By using a composite base material of modified magnesium diboride and epoxy resin and polyester resin in powder coatings, the problems of traditional coating pollution and wear resistance are solved, and the preparation of impact-resistant and wear-resistant powder coatings is realized. Significantly improves the performance and environmental protection of the paint.
Patent Information
- Application Number
- CN202410545544.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-06
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-05-06
AI Technical Summary
The toxic and harmful waste gases and wastewater generated by traditional coatings during use cause pollution to the environment, and the wear and impact resistance of epoxy powder coatings is insufficient, so it cannot be effectively improved by simply adding high-hardness inorganic materials.
Using a composite matrix of epoxy resin and polyester resin, and by modifying magnesium diboride as active filler, it forms modified magnesium diboride through the reaction of silane ethylene, sulfide and aldehyde POSS, and combines with UV. The condensation reaction between light and amine aldehydes improves the compatibility and performance of the resin.
Prepare a powder coating that is impact-resistant and wear-resistant, which significantly improves the hardness, adhesion and high temperature resistance of the coating, reduces environmental pollution, and has better compatibility with the resin, improving The overall performance of the paint.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of powder coatings, and in particular to an impact-resistant and wear-resistant powder coating and a preparation method thereof. Background Art
[0002] Traditional coatings will produce a large amount of toxic and harmful waste gas and wastewater during the manufacturing process or during the use and construction process, which will pollute the environment, atmosphere and water resources. Especially solvent-based coatings will release volatile organic compounds (VOC) into the atmosphere during the construction process, and its amount reaches more than 50%, causing serious secondary pollution. Therefore, as a kind of green and environmentally friendly powder coating, it has been widely used in many fields, especially metal coating in recent years.
[0003] Powder coatings are often based on organic resins such as epoxy, polyester, acrylic, and polyurethane. Among them, epoxy powder coatings are a type of thermosetting powder coatings with excellent adhesion. After spraying and thermal curing on the metal surface, a hard coating is obtained with good anti-corrosion properties. However, epoxy powder coatings have insufficient wear resistance and impact resistance. Technology adds high-hardness inorganic materials to the main resin material to improve the corresponding performance, but the compatibility of inorganic materials with epoxy resin is insufficient, resulting in its performance cannot be effectively improved. Summary of the invention
[0004] In view of the problems existing in the prior art, the object of the present invention is to provide an impact-resistant and wear-resistant powder coating and a preparation method thereof.
[0005] The purpose of the present invention is achieved by adopting the following technical solutions:
[0006] In a first aspect, the present invention provides an impact-resistant and wear-resistant powder coating, calculated by weight, comprising:
[0007] 80-120 parts of epoxy resin, 24-36 parts of polyester resin, 32-48 parts of active filler, 2.1-8.5 parts of pigment, 0.5-1.5 parts of dispersant, 0.8-1.6 parts of defoamer and 15-25 parts of curing agent.
[0008] Preferably, the epoxy resin is bisphenol A epoxy resin, and the models include E51 or E44.
[0009] Preferably, the polyester resin is a hydroxyl-terminated saturated polyester resin with a viscosity of 4500-5500 mPa·s, a relative molecular weight of 6000, and an acid value of 4 mgKOH / g.
[0010] Preferably, the pigment is one or more combinations of Pigment Red 247, Pigment Yellow K1310, and Pigment Blue 60.
[0011] Preferably, the dispersant is one or more combinations of BYK-110, BYK-163, BYK-190 and BYK-161.
[0012] Preferably, the defoaming agent is one or more combinations of Dow Corning AFE-3168, AFE-1520, AFE-1410, and AFE-7610.
[0013] Preferably, the curing agent is one of curing agent BL-3175, curing agent BL-3370, and curing agent BL-3575.
[0014] Preferably, the active filler is modified magnesium diboride, and the preparation method comprises:
[0015] S1. Weigh vinyltrimethoxysilane and mix thoroughly with deionized water, then add magnesium diboride nanopowder, stir at 60-70° C. for 5-10 hours, and after the treatment, filter out the powder, wash with water, and then vacuum dry to obtain vinyl magnesium diboride;
[0016] S2, weighing vinyl magnesium diboride, 4-aminothiophenol and N-methylpyrrolidone, mixing them thoroughly, adding a UV sensitizer, applying UV light, stirring at room temperature for 2-4 hours, and after the treatment, filtering out the powder, washing with alcohol and vacuum drying to obtain aminothioether magnesium diboride;
[0017] S3. Weigh the aldehyde POSS and N,N-dimethylformamide, mix them, heat to 85-95°C for 1-2h, then cool to 60-70°C, add aminothioetherified magnesium diboride, then drop glacial acetic acid, keep warm and stir for 3-5h, remove the solvent under reduced pressure to obtain modified magnesium diboride.
[0018] Preferably, in said S1, the particle size of the magnesium diboride nanopowder is 200-300 nm.
[0019] Preferably, in S1, the mass ratio of magnesium diboride nanopowder, vinyltrimethoxysilane and deionized water is 1:0.2-0.4:10-20.
[0020] Preferably, in S2, the mass ratio of vinyl magnesium diboride, 4-aminothiophenol and N-methylpyrrolidone is 1:0.36-0.72:10-20.
[0021] Preferably, in S2, the ultraviolet sensitizer is one selected from benzoin dimethyl ether, benzoin diethyl ether, and 2,2-diethoxyacetophenone, and the added amount is 5%-8% of the mass of 4-aminothiophenol.
[0022] Preferably, in S3, the mass ratio of aminothioetherified magnesium diboride, aldehyde POSS and N,N-dimethylformamide is 1:3.3-6.6:20-30.
[0023] Preferably, in S3, the amount of glacial acetic acid added is 0.5%-1.5% of the mass of the aldehyde-based POSS.
[0024] Preferably, the preparation method of the aldehyde POSS in S3 comprises:
[0025] Weigh octaphenyl cage silsesquioxane (Ph-POSS, C 48 H 40 O 12 Si 8 ) and 4-chloromethylbenzaldehyde are mixed in N,N-dimethylformamide, stirred thoroughly to dissolve, and then a catalyst is added. The temperature is raised to 60-70°C and stirred for 3-5 hours. After the reaction is completed, the solvent is removed under reduced pressure, and the product is washed with alcohol three times and then dried in vacuum to obtain aldehyde-based POSS.
[0026] Preferably, in the preparation process of the aldehyde-based POSS, the mass ratio of octaphenyl cage silsesquioxane, 4-chloromethylbenzaldehyde and N,N-dimethylformamide is 1:2.3-2.8:20-30.
[0027] Preferably, in the preparation process of the aldehyde-based POSS, the catalyst is aluminum chloride, and the added amount is 20%-30% of the mass of the octaphenyl cage silsesquioxane.
[0028] In a second aspect, the present invention provides a method for preparing an impact-resistant and wear-resistant powder coating, comprising the following steps:
[0029] Weigh all raw materials and mix them in a mixer. After fully mixing, transfer them into a twin-screw extruder and perform melt extrusion to obtain an extrudate. Grind the extrudate in a grinder to obtain an impact-resistant and wear-resistant powder coating.
[0030] Preferably, the temperature of the melt extrusion by the extruder is 115-125° C., and the rotation speed of the extruder is 250-350 r / min.
[0031] Preferably, the powder is ground in the grinder to a particle size of 300-500 mesh.
[0032] The beneficial effects of the present invention are:
[0033] 1. The present invention prepares a powder coating, which uses two composite resins, epoxy resin and polyester resin, as base materials. Epoxy resin has the advantages of high strength, high rigidity and good heat resistance, and polyester resin has the advantages of low cost, good electrical insulation and good processability, which can make up for the shortcomings of epoxy resin to a certain extent. In addition, the filler used in the present invention is modified magnesium diboride, which has better compatibility with the resin after modification, and also has good improvements in the hardness, high temperature resistance, toughness and other aspects of the resin coating.
[0034] 2. The active filler used in the present invention is modified magnesium diboride, which is prepared by sequentially subjecting magnesium diboride nanopowder to silane vinylation, reaction combination with 4-aminothiophenol, and reaction combination with aldehyde POSS to finally obtain a modified coated product containing POSS group, sulfide group, and Schiff base group.
[0035] 3. In the preparation of modified magnesium diboride, during the reaction of 4-aminothiophenol containing both amino and thiol groups with vinyl magnesium diboride, the thiol group and the vinyl group undergo a click chemical reaction under the action of ultraviolet light to form a thioether group coated on the surface of the magnesium diboride to obtain aminothioether magnesium diboride; then, it combines with the aldehyde group POSS, and the amino group on the surface of the aminothioether magnesium diboride undergoes an amine-aldehyde condensation reaction with the aldehyde group to form a Schiff base group, thereby finally obtaining modified magnesium diboride.
[0036] 4. The preparation of aldehyde POSS (CHO-POSS) is carried out by using octaphenyl cage silsesquioxane (Ph-POSS) and 4-chloromethylbenzaldehyde as reactants, and a Friedel-Crafts reaction is carried out under the catalysis of aluminum chloride to graft aldehyde groups on the POSS groups to obtain CHO-POSS. DETAILED DESCRIPTION
[0037] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.
[0038] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0039] The water washing in the present invention is all pure water washing, and the alcohol washing is all ethanol washing.
[0040] The present invention will be further described below in conjunction with the following examples.
[0041] Example 1
[0042] An impact-resistant and wear-resistant powder coating, calculated by weight, comprising:
[0043] 100 parts epoxy resin, 30 parts polyester resin, 40 parts active filler, 5.3 parts pigment, 1 part dispersant, 1.2 parts defoamer and 20 parts curing agent.
[0044] The epoxy resin is bisphenol A epoxy resin, model E51; the polyester resin is a hydroxyl-terminated saturated polyester resin, with a viscosity of 4500-5500 mPa·s, a relative molecular weight of 6000, and an acid value of 4 mgKOH / g.
[0045] The pigment is BASF Pigment Yellow K1310; the dispersant is BYK-110; the defoamer is Dow Corning AFE-3168; and the curing agent is curing agent BL-3175.
[0046] The active filler is modified magnesium diboride, and the preparation method includes:
[0047] S1. Weigh vinyl trimethoxysilane and mix it thoroughly with deionized water, then add magnesium diboride nanopowder with a particle size of 200-300 nm, the mass ratio of magnesium diboride nanopowder, vinyl trimethoxysilane and deionized water is 1:0.3:15, stir at 65 ° C for 8 hours, after the treatment is completed, filter out the powder, wash with water and then vacuum dry to obtain vinyl magnesium diboride;
[0048] S2, weighing vinyl magnesium diboride, 4-aminothiophenol and N-methylpyrrolidone and mixing them thoroughly, the mass ratio of vinyl magnesium diboride, 4-aminothiophenol and N-methylpyrrolidone is 1:0.54:15, and then adding ultraviolet photosensitizer benzoin dimethyl ether, the addition amount is 6% of the mass of 4-aminothiophenol, applying ultraviolet light with a wavelength of 254nm, stirring at room temperature for 3h, after the treatment is completed, filtering out the powder, washing with alcohol and vacuum drying to obtain aminothioether magnesium diboride;
[0049] S3, weigh octaphenyl cage silsesquioxane (Ph-POSS, C 48 H 40 O 12 Si 8 ) and 4-chloromethylbenzaldehyde are mixed in N,N-dimethylformamide, the mass ratio of octaphenyl cage silsesquioxane, 4-chloromethylbenzaldehyde and N,N-dimethylformamide is 1:2.5:25, after fully stirring and dissolving, adding catalyst aluminum chloride, the addition amount is 25% of the mass of octaphenyl cage silsesquioxane, heating to 65°C, stirring for 4h, after the reaction is completed, removing the solvent under reduced pressure, washing with alcohol three times and vacuum drying to obtain aldehyde-based POSS;
[0050] S4. Weigh aldehyde POSS and N,N-dimethylformamide, mix them, heat to 90°C and treat for 1.5h, then cool to 65°C, add aminothioetherified magnesium diboride, the mass ratio of aminothioetherified magnesium diboride, aldehyde POSS and N,N-dimethylformamide is 1:4.9:25, then drop glacial acetic acid, the amount of glacial acetic acid added is 1% of the mass of aldehyde POSS, keep warm and stir for 4h, remove the solvent under reduced pressure to obtain modified magnesium diboride.
[0051] The method for preparing the above-mentioned impact-resistant and wear-resistant powder coating comprises the following steps:
[0052] Weigh all the raw materials and mix them in a mixer. After fully mixing, transfer them into a twin-screw extruder at a speed of 300r / min. After melt extrusion at 115-125°C, obtain an extrudate. Grind the extrudate in a grinder to obtain an impact-resistant and wear-resistant powder coating of 300-500 mesh.
[0053] Example 2
[0054] An impact-resistant and wear-resistant powder coating, calculated by weight, comprising:
[0055] 80 parts of epoxy resin, 24 parts of polyester resin, 32 parts of active filler, 2.1 parts of pigment, 0.5 parts of dispersant, 0.8 parts of defoamer and 15 parts of curing agent.
[0056] The epoxy resin is bisphenol A epoxy resin, model E44; the polyester resin is a hydroxyl-terminated saturated polyester resin, with a viscosity of 4500-5500 mPa·s, a relative molecular weight of 6000, and an acid value of 4 mgKOH / g.
[0057] The pigment is Clariant Pigment Red 247; the dispersant is BYK-163; the defoamer is Dow Corning AFE-1520; and the curing agent is curing agent BL-3370.
[0058] The active filler is modified magnesium diboride, and the preparation method includes:
[0059] S1. Weigh vinyl trimethoxysilane and mix it thoroughly with deionized water, then add magnesium diboride nanopowder with a particle size of 200-300 nm, the mass ratio of magnesium diboride nanopowder, vinyl trimethoxysilane and deionized water is 1:0.2:10, stir at 60°C for 5h, after the treatment, filter out the powder, wash with water and then vacuum dry to obtain vinyl magnesium diboride;
[0060] S2, weighing vinyl magnesium diboride, 4-aminothiophenol and N-methylpyrrolidone and mixing them thoroughly, the mass ratio of vinyl magnesium diboride, 4-aminothiophenol and N-methylpyrrolidone is 1:0.36:10, and then adding ultraviolet sensitizer benzoin diethyl ether, the addition amount is 5% of the mass of 4-aminothiophenol, applying ultraviolet light, stirring at room temperature for 2h, after the treatment is completed, filtering out the powder, washing with alcohol and vacuum drying to obtain aminothioether magnesium diboride;
[0061] S3, weigh octaphenyl cage silsesquioxane (Ph-POSS, C 48 H 40 O 12 Si 8 ) and 4-chloromethylbenzaldehyde are mixed in N,N-dimethylformamide, the mass ratio of octaphenyl cage silsesquioxane, 4-chloromethylbenzaldehyde and N,N-dimethylformamide is 1:2.3:20, after fully stirring and dissolving, adding catalyst aluminum chloride, the addition amount is 20% of the mass of octaphenyl cage silsesquioxane, heating to 60°C, stirring for 3h, after the reaction is completed, removing the solvent under reduced pressure, washing with alcohol three times and vacuum drying to obtain aldehyde-based POSS;
[0062] S4. Weigh aldehyde POSS and N,N-dimethylformamide, mix them, heat to 85°C for 1h, then cool to 60°C, add aminothioetherified magnesium diboride, the mass ratio of aminothioetherified magnesium diboride, aldehyde POSS and N,N-dimethylformamide is 1:3.3:20, then drop glacial acetic acid, the amount of glacial acetic acid added is 0.5% of the mass of aldehyde POSS, keep warm and stir for 3h, remove the solvent under reduced pressure to obtain modified magnesium diboride.
[0063] The method for preparing the above-mentioned impact-resistant and wear-resistant powder coating comprises the following steps:
[0064] Weigh all the raw materials and mix them in a mixer. After fully mixing, transfer them into a twin-screw extruder at a speed of 300r / min. After melt extrusion at 115-125°C, obtain an extrudate. Grind the extrudate in a grinder to obtain an impact-resistant and wear-resistant powder coating of 300-500 mesh.
[0065] Example 3
[0066] An impact-resistant and wear-resistant powder coating, calculated by weight, comprising:
[0067] 120 parts of epoxy resin, 36 parts of polyester resin, 48 parts of active filler, 8.5 parts of pigment, 1.5 parts of dispersant, 1.6 parts of defoamer and 25 parts of curing agent.
[0068] The epoxy resin is bisphenol A epoxy resin, and the model includes E51; the polyester resin is a hydroxyl-terminated saturated polyester resin, and has a viscosity of 4500-5500 mPa·s, a relative molecular weight of 6000, and an acid value of 4 mgKOH / g.
[0069] The pigment is Pigment Blue 60; the dispersant is BYK-190; the defoamer is Dow Corning AFE-7610; and the curing agent is curing agent BL-3575.
[0070] The active filler is modified magnesium diboride, and the preparation method includes:
[0071] S1. Weigh vinyl trimethoxysilane and mix it thoroughly with deionized water, then add magnesium diboride nanopowder with a particle size of 200-300 nm, the mass ratio of magnesium diboride nanopowder, vinyl trimethoxysilane and deionized water is 1:0.4:20, stir at 70°C for 10 hours, after the treatment is completed, filter out the powder, wash with water and then vacuum dry to obtain vinyl magnesium diboride;
[0072] S2, weighing vinyl magnesium diboride, 4-aminothiophenol and N-methylpyrrolidone and mixing them thoroughly, the mass ratio of vinyl magnesium diboride, 4-aminothiophenol and N-methylpyrrolidone is 1:0.72:20, and then adding ultraviolet sensitizer 2,2-diethoxyacetophenone, the addition amount is 8% of the mass of 4-aminothiophenol, applying ultraviolet light, stirring at room temperature for 4h, after the treatment is completed, filtering out the powder, washing with alcohol and vacuum drying to obtain aminothioether magnesium diboride;
[0073] S3, weigh octaphenyl cage silsesquioxane (Ph-POSS, C 48 H 40 O 12 Si 8 ) and 4-chloromethylbenzaldehyde are mixed in N,N-dimethylformamide, the mass ratio of octaphenyl cage silsesquioxane, 4-chloromethylbenzaldehyde and N,N-dimethylformamide is 1:2.8:30, after fully stirring and dissolving, adding catalyst aluminum chloride, the addition amount is 30% of the mass of octaphenyl cage silsesquioxane, heating to 70°C, stirring for 5h, after the reaction is completed, removing the solvent under reduced pressure, washing with alcohol three times and vacuum drying to obtain aldehyde-based POSS;
[0074] S4. Weigh aldehyde POSS and N,N-dimethylformamide, mix them, heat to 95°C and treat for 2h, then cool to 70°C, add aminothioetherified magnesium diboride, the mass ratio of aminothioetherified magnesium diboride, aldehyde POSS and N,N-dimethylformamide is 1:6.6:30, then drop glacial acetic acid, the amount of glacial acetic acid added is 1.5% of the mass of aldehyde POSS, keep warm and stir for 5h, remove the solvent under reduced pressure to obtain modified magnesium diboride.
[0075] The method for preparing the above-mentioned impact-resistant and wear-resistant powder coating comprises the following steps:
[0076] Weigh all the raw materials and mix them in a mixer. After fully mixing, transfer them into a twin-screw extruder at a speed of 350r / min. After melt extrusion at 115-125°C, obtain an extrudate. Grind the extrudate in a grinder to obtain an impact-resistant and wear-resistant 300-500 mesh powder coating.
[0077] Comparative Example 1
[0078] An impact-resistant and wear-resistant powder coating, which differs from Example 1 only in that the active filler is replaced by vinyl magnesium diboride (prepared in the same manner as step S1 of Example 1).
[0079] Comparative Example 2
[0080] An impact-resistant and wear-resistant powder coating, which differs from Example 1 in that the active filler is replaced by aminothioetherified magnesium diboride (prepared in the same steps S1 and S2 of Example 1).
[0081] Comparative Example 3
[0082] An impact-resistant and wear-resistant powder coating, which differs from Example 1 in that the active filler is replaced by a mixture of vinyl magnesium diboride (prepared in the same manner as step S1 of Example 1) and octaphenyl cage silsesquioxane (Ph-POSS) in a mass ratio of 1:6.6.
[0083] Experimental testing
[0084] Experimental tests were carried out on the powder coatings prepared in Example 1 and Comparative Examples 1-3 to illustrate their performance.
[0085] Experimental preparation: The powder coatings prepared in Example 1 and Comparative Examples 1-3 were sprayed on 304 stainless steel plates respectively with a spraying thickness of 100±5 μm, and then kept at 150° C. for half an hour to allow it to fuse and solidify, and then its performance was tested.
[0086] Test content: Hardness test is the pencil method, refer to GB / T 9754-2007; impact resistance test is based on GB / T1732-2020; adhesion test is based on GB / T 9286-2012; high temperature resistance is the change in total color difference △E after treatment at 300℃ for 10h, refer to GB / T 1735-2009.
[0087] The test results are shown in Table 1:
[0088] Table 1 Performance of different powder coatings
[0089]
[0090] It can be seen from Table 1 that the hardness, adhesion and impact resistance of the powder coating prepared in Example 1 are all better, and the color difference ΔE after high temperature treatment is the smallest, indicating that it has better high temperature resistance.
[0091] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.
[0092] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. An impact-resistant and wear-resistant powder coating, characterized in that: Calculated by weight, including: 80-120 parts of epoxy resin, 24-36 parts of polyester resin, 32-48 parts of active filler, 2.1-8.5 parts of pigment, 0.5-1.5 parts of dispersant, 0.8-1.6 parts of defoamer and 15-25 parts of curing agent; The active filler is modified magnesium diboride, and the preparation method comprises: S1. Weigh vinyltrimethoxysilane and mix thoroughly with deionized water, then add magnesium diboride nanopowder, stir at 60-70° C. for 5-10 hours, and after the treatment, filter out the powder, wash with water, and then vacuum dry to obtain vinyl magnesium diboride; S2, weighing vinyl magnesium diboride, 4-aminothiophenol and N-methylpyrrolidone, mixing them thoroughly, adding a UV sensitizer, applying UV light, stirring at room temperature for 2-4 hours, and after the treatment, filtering out the powder, washing with alcohol and vacuum drying to obtain aminothioether magnesium diboride; S3, weighing aldehyde POSS and N, N-dimethylformamide, mixing, heating to 85-95 ° C for 1-2h, then cooling to 60-70 ° C, adding aminothioetherified magnesium diboride, and then dropping glacial acetic acid, keeping warm and stirring for 3-5h, removing the solvent under reduced pressure to obtain modified magnesium diboride; The epoxy resin is a bisphenol A epoxy resin, and the model includes E51 or E44; the polyester resin is a hydroxyl-terminated saturated polyester resin, and the viscosity is 4500-5500 mPa·s, the relative molecular weight is 6000, and the acid value is 4 mgKOH / g; The curing agent is one of curing agent BL-3175, curing agent BL-3370, and curing agent BL-3575; In S1, the mass ratio of magnesium diboride nanopowder, vinyltrimethoxysilane and deionized water is 1:0.2-0.4:10-20; In S2, the mass ratio of vinyl magnesium diboride, 4-aminothiophenol and N-methylpyrrolidone is 1:0.36-0.72:10-20; the ultraviolet sensitizer is one selected from benzoin dimethyl ether, benzoin diethyl ether, and 2,2-diethoxyacetophenone, and the added amount is 5%-8% of the mass of 4-aminothiophenol; In S3, the mass ratio of aminothioetherified magnesium diboride, aldehyde POSS and N,N-dimethylformamide is 1:3.3-6.6:20-30; and the amount of glacial acetic acid added is 0.5%-1.5% of the mass of aldehyde POSS.
2. The impact-resistant and wear-resistant powder coating according to claim 1, characterized in that: The pigment is one or more combinations of Pigment Red 247, Pigment Yellow K1310, and Pigment Blue 60.
3. The impact-resistant and wear-resistant powder coating according to claim 1, characterized in that: The dispersant is one or more combinations of BYK-110, BYK-163, BYK-190, and BYK-161; the defoamer is one or more combinations of Dow Corning AFE-3168, AFE-1520, AFE-1410, and AFE-7610.
4. A method for preparing the impact-resistant and wear-resistant powder coating according to claim 1, characterized in that: The following steps are involved: Weigh all raw materials and mix them in a mixer. After fully mixing, transfer them into a twin-screw extruder and perform melt extrusion to obtain an extrudate. Grind the extrudate in a grinder to obtain an impact-resistant and wear-resistant powder coating.