Processing technology of high temperature low alloy steel track shoes
By using DC arc plasma technology to prepare microcrystalline carbide on the track pad and combining it with modified resin treatment, the problems of insufficient hardness, wear resistance and high temperature resistance of the track pad are solved, and its performance is significantly improved, including hardness, resistance and resistance. Abrasion and corrosion resistance.
Patent Information
- Application Number
- CN202410912139.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-09
AI Technical Summary
The existing high temperature low alloy steel track shoes have poor hardness, wear resistance, high temperature resistance and corrosion resistance.
DC arc plasma technology is used to prepare microcrystalline carbide, which is added as an additive to the mixed powder, combined with modified resin and polyisocyanate curing agent, and then coated on the track plate through normalizing, quenching and tempering treatments. Surface, forming high-temperature low-alloy steel track shoes with excellent performance.
Significantly improves the hardness, wear resistance and high temperature resistance of the track pad, while enhancing its corrosion resistance and extending its service life.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of track plate processing, and in particular relates to a processing technology of a high-temperature low-alloy steel track plate. Background Art
[0002] With the continuous development of modern industrial technology, the performance requirements for track shoes are becoming increasingly stringent, especially under extreme working conditions such as high temperature, heavy load, and complex terrain. Track shoes need to have higher strength, toughness, wear resistance, and fatigue resistance. As a special metal material, high temperature low alloy steel has excellent high temperature performance and low alloy element content, and is an ideal material for manufacturing track shoes. However, due to its special chemical composition and microstructure, the processing technology of high temperature low alloy steel is relatively complex, and it is necessary to fully consider the thermal deformation behavior, phase change law, and the relationship between organization and performance of the material. In addition, as an important component for bearing and transmitting power, the processing accuracy and surface quality of the track shoe have an important influence on the overall performance of the equipment. Therefore, studying the processing technology of high temperature low alloy steel track shoes is of great significance for improving the performance of track shoes, reducing production costs, and meeting market demand.
[0003] Patent CN 112813362 B discloses a method for manufacturing high-strength steel and a high-strength steel track plate, including smelting, rolling, and fine forging processes. In the smelting process, the chemical composition of the high-strength steel embryo body includes: carbon, silicon, manganese, chromium, molybdenum, rhenium, nickel, sulfur, phosphorus, and the rest is Fe and inevitable impurities; including smelting the raw materials by an electric arc furnace or a medium frequency induction furnace to obtain molten steel; LF refining and VD vacuum treatment of the molten steel in sequence; pouring the refined molten steel into an ingot mold to obtain an ingot, or pouring it into a continuous casting crystallizer to obtain a continuous casting embryo. The high-strength steel provided by the invention has high strength and high toughness, and the high-strength steel track plate provided solves the problem that the track plate has low low-temperature impact toughness and is easy to break when used in high-cold areas. However, the hardness, wear resistance, high temperature resistance and corrosion resistance of the track plate obtained by this method still have room for improvement. Summary of the invention
[0004] The purpose of the present invention is to provide a processing technology for high-temperature low-alloy steel track shoes, which is used to solve the technical problems of poor hardness, wear resistance, high temperature resistance and corrosion resistance of track shoes in the prior art.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The present invention provides a processing technology for high temperature low alloy steel track shoe, comprising the following steps:
[0007] Step (1): ball-milling and mixing Fe, Si, Mn, Cr, Ni, Mo and microcrystalline carbides to obtain a low alloy mixture;
[0008] Step (2): subjecting the low alloy mixture to temperature normalizing, temperature quenching, high temperature tempering, surface quenching and low temperature tempering treatments to obtain a low alloy crude product;
[0009] Step (3): The modified resin and the polyisocyanate curing agent are stirred and mixed, applied to the surface of the low alloy crude product, and cured to obtain a high temperature low alloy steel track shoe.
[0010] Preferably, in step (1), the mass ratio of Fe, Si, Mn, Cr, Ni, Mo and microcrystalline carbide is (95.55-96.45): (0.45-0.85): (1.15-1.55): (0.85-1.05): (0.75-1.15): (0.25-0.45): (0.035-0.075), and during the ball milling mixing process, the ball milling medium is stainless steel balls, the ball milling time is 20-30 hours, and the ball milling speed is 300-400 rpm.
[0011] Preferably, the method for preparing the microcrystalline carbide comprises the following steps:
[0012] Q1: Grind carbon powder and niobium powder in a mortar until they are evenly mixed and have similar particle sizes. Place the mixed material in a tablet press for tableting to obtain thin discs.
[0013] Q2: Place the graphite pot with thin discs into a water-cooled copper pot, use a tungsten rod as the cathode material, and fix the graphite pot as the anode material in a DC arc meter. Seal it with a columnar glass cover, start the power supply, and after the reaction is completed, turn off the power supply and passivate it in a nitrogen atmosphere. After passivation, collect the material on the graphite pot to obtain microcrystalline carbide.
[0014] In the above process, carbon powder and niobium powder are used as raw materials to prepare microcrystalline carbide using DC arc plasma technology. In the DC arc instrument, after the power is turned on, an arc is generated between the tungsten rod and the graphite pot, thereby generating high temperature, causing nitrogen to be ionized to form plasma. The high temperature environment generated by the arc causes the carbon powder and niobium powder to be rapidly heated, and the carbon atoms and niobium atoms become active, undergoing chemical reactions to generate microcrystalline carbides.
[0015] Preferably, in Q1, the molar ratio of carbon powder to niobium powder is (0.9-1.1): (0.9-1.1), and during the tableting process, the applied pressure is 150-170 MPa for 3-5 min. In Q2, after starting the power supply, the vacuum pump is turned on to evacuate the air in the glass cover. When the air pressure is less than 10 Pa, the vacuum pump is temporarily turned off, and 30-50 kPa of nitrogen is slowly introduced, and the air is evacuated again. After the evacuation is completed, 40 kPa of nitrogen is filled, the water cooling circulation system is started, the DC arc welding machine is turned on, the current of the arc welding machine is adjusted to 100 A, and the reaction is carried out for 8-10 min after the arc is generated. The reaction is completed and the passivation time is 3-4 h.
[0016] Preferably, in step (2), the temperature of normalizing is 800-950°C, the temperature of quenching is 850-920°C, the temperature of high temperature tempering is 550-650°C, the temperature of surface quenching is 850-900°C, and the temperature of low temperature tempering is 150-200°C.
[0017] Preferably, in step (3), the method for preparing the modified resin comprises the following steps:
[0018] S1: adding anhydrous ethanol and phosphorus pentoxide to a container under ice water bath conditions, stirring and mixing evenly, heating the system, and continuing to stir and react, then adding deionized water for hydrolysis reaction, and after the reaction is completed, cooling to obtain a phosphate compound;
[0019] S2: Add methyltrimethoxysilane, dimethyldimethoxysilane, hexamethyldisilane and anhydrous ethanol into a container equipped with a reflux condenser, a thermometer and a dropping funnel, stir the mixed liquid, heat and raise the temperature, add deionized water for hydrolysis reaction, and dropwise add hydrochloric acid. After the dropwise addition is completed, heat and react at a constant temperature, then dropwise add butyl titanate dissolved in xylene, add deionized water after the dropwise addition is completed, hydrolyze, distill under reduced pressure, and heat and condense to obtain a titanium-containing compound;
[0020] S3: adding neopentyl glycol, trimethylolpropane and diethylene glycol to a container containing a thermometer, a reflux condenser, a water separator and a stirrer, introducing nitrogen, heating and stirring, then adding isophthalic acid, xylene and dibutyltin dilaurate, heating to react, then continuing to heat to react, after the reaction is completed, cooling and adding sebacic acid, continuing to heat to react, after the reaction is completed, cooling, adding xylene to dilute, and obtaining a polyester resin;
[0021] S4: adding a phosphoric acid compound to the polyester resin, heating and stirring to react, then adding a titanium-containing compound and dibutyltin dilaurate, after the addition is complete, heating to react, after the reaction is completed, cooling and discharging to obtain a modified resin.
[0022] In the above process, anhydrous ethanol and phosphorus pentoxide undergo an esterification reaction to obtain a phosphoric acid compound; methyltrimethoxysilane, dimethyldimethoxysilane, and hexamethyldisilane react with deionized water to hydrolyze the silane to generate silanol, which then undergoes a condensation reaction to obtain a titanium-containing compound; neopentyl glycol, trimethylolpropane, and diethylene glycol undergo an esterification reaction with isophthalic acid to obtain a polyester resin; under the catalytic action of dibutyltin dilaurate, the phosphoric acid compound, the polyester resin, and the titanium-containing compound react to obtain a modified resin.
[0023] Preferably, in S1, the molar ratio of anhydrous ethanol to phosphorus pentoxide is (3.8-4.2): (0.8-1.1), the heating temperature is 75-80°C, the stirring reaction time is 3-4h, and the hydrolysis reaction time is 2-3h; in S2, the amount ratio of methyltrimethoxysilane, dimethyldimethoxysilane, hexamethyldisilane, anhydrous ethanol, deionized water, xylene and butyl titanate is (9.34-9.76) g: (8.64-8.78) g: (9.21-9.35) g: (38-42) mL: (7-10) mL: (30-35) mL: (20-24) mL, the heating temperature is 60-70°C, the constant temperature heating reaction time is 2-3h, the hydrolysis time is 3-4h, the heating condensation temperature is 120-130°C, and the time is 2-3h.
[0024] Preferably, in S3, the mass ratio of neopentyl glycol, trimethylolpropane, diethylene glycol, isophthalic acid and sebacic acid is (27.52-27.92) g: (8.14-8.42) g: (27.45-28.23) g: (48.71-49.01) g: (11.22-11.44) g, the heating and stirring temperature is 130-140°C, the time is 30-40 min, the heating reaction temperature is 170-180°C, and the time is 4-5 h. The temperature of the reaction is continued to rise to 210-220°C for 6-8h, the temperature is cooled to 160-170°C, the temperature of the reaction is continued to rise to 200-210°C for 2-3h; in S4, the volume ratio of the phosphate compound, the polyester resin and the titanium-containing compound is (18-22) mL: (13-15) mL: (9-13) mL, the heating and stirring reaction temperature is 75-85°C for 2-2.5h, the heating reaction temperature is 170-180°C for 1-2h.
[0025] Preferably, in step (3), the ratio of the modified resin to the polyisocyanate curing agent is (20-30) mL: (2-5) mL, the stirring mixing time is 20-30 min, the surface of the crude low alloy product is first cleaned with acetone and ethanol, and then coated after drying, the curing temperature is 150-180°C, and the time is 10-15 min.
[0026] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0027] 1. The present invention firstly utilizes direct current arc plasma technology to prepare microcrystalline carbide, which can be used as an additive to effectively improve the hardness, wear resistance and high temperature resistance of the track plate. However, the addition of microcrystalline carbide will affect the toughness of the track plate. Coating the modified resin on the surface of the track plate can not only reduce the effect of microcrystalline carbide on toughness, but also improve the corrosion resistance of the track plate. Therefore, the high-temperature low-alloy steel track plate prepared by this method has excellent hardness, wear resistance, high temperature resistance and corrosion resistance.
[0028] 2. The present invention uses carbon powder and niobium powder as raw materials, prepares microcrystalline carbide by DC arc plasma technology, and adds the substance as an additive to the mixed powder. The prepared track plate has excellent hardness, wear resistance and high temperature resistance. This is mainly because the microcrystalline carbide itself has a very high hardness. When added to the mixed powder, it plays the role of a "reinforcement phase", thereby improving the hardness of the entire material; the excellent wear resistance of the microcrystalline carbide enables the track plate containing it to resist more external forces when facing friction and wear, thereby extending its service life; and its excellent high temperature resistance enables the track plate to still maintain good physical properties and service life in a high temperature environment.
[0029] 3. The present invention uses phosphorus pentoxide, methyltrimethoxysilane, neopentyl glycol, trimethylolpropane, and isophthalic acid as raw materials to prepare a modified resin, which is mixed with a polyisocyanate curing agent and coated on the surface of a low-alloy crude product. After curing, a high-temperature low-alloy steel track plate with excellent corrosion resistance is obtained. Anhydrous ethanol and phosphorus pentoxide are first esterified to generate a phosphoric acid compound, which forms a dense protective film on the surface of the track plate, effectively isolating the corrosive medium and significantly improving the corrosion resistance; at the same time, silane is hydrolyzed and condensed to generate a titanium-containing compound, which can form a corrosion-resistant titanium-based coating on the surface of the material to further protect the substrate; under the catalysis of dibutyltin dilaurate, the phosphoric acid compound, polyester resin and titanium-containing compound react to form a modified resin, which not only enhances the corrosion resistance of the coating, but also forms a strong chemical bond with the metal surface through its functional groups, thereby improving the corrosion resistance. The adhesion and corrosion resistance of the coating are improved, so that the track shoe has excellent corrosion resistance; the synthesized polyester resin has good toughness and ductility. When it is applied to the surface of the track shoe as a coating, it can effectively absorb external impact and vibration energy, reduce the stress concentration and crack propagation of the material, thereby improving the toughness of the track shoe; the modified resin obtained will form a three-dimensional cross-linked network structure during the curing process, which effectively constrains the molecular movement of the material and improves the cohesion and toughness of the material. The applied coating also has the effect of buffering and vibration reduction, which can improve the toughness and service life of the track shoe. DETAILED DESCRIPTION
[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The chemical reagents used in the examples and comparative examples are all commercially available products, and the manufacturers and CAS numbers are as follows:
[0032] Toner was purchased from Beijing Ruichi High-Tech Co., Ltd., CAS No.: 7440-44-0;
[0033] Niobium powder was purchased from Hebei Yuechao Wear Resistant Materials Co., Ltd., CAS No.: 7440-03-1;
[0034] Anhydrous ethanol was purchased from Foshan Changxing New Materials Co., Ltd., CAS No.: 64-17-5;
[0035] Phosphorus pentoxide was purchased from Shandong Xuchen Chemical Technology Co., Ltd., CAS No.: 1314-56-3;
[0036] Methyltrimethoxysilane was purchased from Shanghai Haiqu Chemical Co., Ltd., CAS No.: 1185-55-3;
[0037] Dimethyldimethoxysilane was purchased from Hangzhou Jessica Chemical Co., Ltd., CAS No.: 1112-39-6;
[0038] Hexamethyldisilane was purchased from Shandong Yuanjin New Materials Co., Ltd., CAS No.: 1450-14-2;
[0039] Hydrochloric acid was purchased from Nanjing Shengqinghe Chemical Co., Ltd., CAS No.: 7647-01-0;
[0040] Xylene was purchased from Jinan Zesheng Chemical Co., Ltd., CAS number: 95-47-6;
[0041] Butyl titanate was purchased from Jiaxiang County Dahai Chemical Co., Ltd., CAS No.: 5593-70-4;
[0042] Neopentyl glycol was purchased from Zibo Anhao Chemical Co., Ltd., CAS No.: 126-30-7;
[0043] Trimethylolpropane was purchased from Shandong Shengteng Chemical Co., Ltd., CAS No.: 77-99-6;
[0044] Diethylene glycol was purchased from Guangzhou Qixu Chemical Co., Ltd., CAS No.: 111-46-6;
[0045] Isophthalic acid was purchased from Shandong Zhijia Chemical Technology Co., Ltd., CAS No.: 121-91-5;
[0046] Dibutyltin dilaurate was purchased from Jinan Pulaihua Chemical Co., Ltd., CAS No.: 77-58-7;
[0047] Sebacic acid was purchased from Handan Tengke Chemical Distribution Co., Ltd., CAS No.: 111-20-6;
[0048] Fe was purchased from Shandong Jinyueyuan New Materials Co., Ltd., CAS No.: 7439-89-6;
[0049] Si was purchased from Shanghai MacLean Biochemical Technology Co., Ltd., CAS No.: 7440-21-3;
[0050] Mn was purchased from Shanghai Jizhi Biochemical Technology Co., Ltd., CAS No.: 7439-96-5;
[0051] Cr was purchased from Hebei Zhentian Food Additive Co., Ltd., CAS No.: 7440-47-3;
[0052] Ni was purchased from Guangdong Wengjiang Chemical Reagent Co., Ltd., CAS No.: 7440-02-0;
[0053] Mo was purchased from Qianyan Chemical Technology (Wuhan) Co., Ltd., CAS No.: 7439-98-7;
[0054] Polyisocyanate curing agent was purchased from Shanghai Kaiyin Chemical Co., Ltd.;
[0055] Acetone was purchased from Maoming Runjing Chemical Co., Ltd., CAS No.: 67-64-1. Example 1
[0056] This embodiment discloses a method for preparing microcrystalline carbide, comprising the following steps:
[0057] Q1: 1.11g carbon powder and 8.61g niobium powder were fully ground in a mortar to make them uniform and of similar particle size. The mixed material was placed in a tablet press for tableting at 150MPa for 5min to obtain a thin disc;
[0058] Q2: Put the graphite pot with thin discs into a water-cooled copper pot, use tungsten rod as cathode material, and fix the graphite pot as anode material in a DC arc instrument, seal it with a columnar glass cover, start the power supply, turn on the vacuum pump to evacuate the air in the glass cover, when the air pressure is less than 10Pa, temporarily turn off the vacuum pump, slowly pass 40kPa of nitrogen, and evacuate again. After the evacuation is completed, fill in 40kPa of nitrogen, start the water-cooled circulation system, turn on the DC arc welder, adjust the current of the arc welder to 100A, react for 10 minutes after the arc is generated, and when the reaction is over, turn off the power supply and passivate for 4 hours in a nitrogen atmosphere. After passivation, collect the substances on the graphite pot to obtain microcrystalline carbide.
[0059] This embodiment discloses a method for preparing a modified resin, comprising the following steps:
[0060] S1: Add 2.053 mL of anhydrous ethanol and 1.188 g of phosphorus pentoxide to a container under ice water bath conditions, stir and mix evenly, then heat the system to 80°C, continue stirring and react for 4 hours, then add deionized water to carry out hydrolysis reaction for 3 hours. After the reaction is completed, cool down to obtain a phosphate compound;
[0061] S2: 9.55 g of methyltrimethoxysilane, 8.71 g of dimethyldimethoxysilane, 9.28 g of hexamethyldisilane and 40 mL of anhydrous ethanol are added to a container equipped with a reflux condenser, a thermometer and a dropping funnel, the mixed liquid is stirred, heated to 60°C, 8.5 mL of deionized water is added for hydrolysis reaction, and hydrochloric acid is added dropwise. After the addition is completed, the reaction is heated at a constant temperature for 3 hours, and 22 mL of butyl titanate dissolved in 32.5 mL of xylene is added dropwise. After the addition is completed, 3 mL of deionized water is added, hydrolysis is carried out for 4 hours, and vacuum distillation is carried out. The temperature is raised to 130°C for condensation for 2 hours to obtain a titanium-containing compound;
[0062] S3: 27.72 g of neopentyl glycol, 8.28 g of trimethylolpropane and 27.84 g of diethylene glycol were added to a container containing a thermometer, a reflux condenser, a water separator and a stirrer, and after nitrogen was introduced, the temperature was raised to 140° C. and stirred for 40 min, and then 48.86 g of isophthalic acid, 20 mL of xylene and dibutyltin dilaurate were added, and the temperature was raised to 180° C. for reaction for 5 h, and then the temperature was continued to be raised to 220° C. for reaction for 6 h. After the reaction was completed, the temperature was lowered to 160° C. and 11.33 g of sebacic acid was added, and the temperature was continued to be raised to 210° C. for reaction for 3 h. After the reaction was completed, the temperature was cooled, and 18 mL of xylene was added for dilution to obtain a polyester resin;
[0063] S4: Add 20 mL of phosphoric acid compound to 14 mL of polyester resin, heat to 85°C and stir to react for 2.5 hours, then add 11 mL of titanium-containing compound and dibutyltin dilaurate. After the addition is complete, heat to 170°C and react for 2 hours. After the reaction is completed, cool and discharge to obtain a modified resin.
[0064] This embodiment discloses a processing technology for a high temperature low alloy steel track shoe, comprising the following steps:
[0065] Step (1): 95.695 g Fe, 0.65 g Si, 1.35 g Mn, 0.95 g Cr, 0.95 g Ni, 0.35 g Mo and 0.055 g microcrystalline carbide are ball-milled, wherein the ball-milling medium is stainless steel balls, the ball-milling time is 23 h, and the ball-milling speed is 400 rpm, to obtain a low alloy mixture;
[0066] Step (2): heating the low alloy mixture to 900°C for normalizing, heating to 920°C for quenching, high temperature tempering at 650°C, surface quenching at 900°C and low temperature tempering at 200°C to obtain a low alloy crude product;
[0067] Step (3): 25 mL of the modified resin and 3.5 mL of the polyisocyanate curing agent were stirred and mixed for 30 minutes, and then coated on the surface of the low-alloy crude product. The surface of the low-alloy crude product was first cleaned with acetone and ethanol, and then coated after drying. The product was cured at 180° C. for 15 minutes to obtain a high-temperature low-alloy steel track shoe. Example 2
[0068] This embodiment discloses a method for preparing microcrystalline carbide, comprising the following steps:
[0069] Q1: 1.00g carbon powder and 7.75g niobium powder were fully ground in a mortar to make them uniform and of similar particle size. The mixed material was placed in a tablet press for tableting at 150MPa for 5min to obtain a thin disc;
[0070] Q2: Put the graphite pot with thin discs into a water-cooled copper pot, use tungsten rod as cathode material, and fix the graphite pot as anode material in a DC arc instrument, seal it with a columnar glass cover, start the power supply, turn on the vacuum pump to evacuate the air in the glass cover, when the air pressure is less than 10Pa, temporarily turn off the vacuum pump, slowly pass 40kPa of nitrogen, and evacuate again. After the evacuation is completed, fill in 40kPa of nitrogen, start the water-cooled circulation system, turn on the DC arc welder, adjust the current of the arc welder to 100A, react for 10 minutes after the arc is generated, and when the reaction is over, turn off the power supply and passivate for 4 hours in a nitrogen atmosphere. After passivation, collect the substances on the graphite pot to obtain microcrystalline carbide.
[0071] This embodiment discloses a method for preparing a modified resin, comprising the following steps:
[0072] S1: Add 1.95 mL of anhydrous ethanol and 1.375 g of phosphorus pentoxide to a container under ice water bath conditions, stir and mix evenly, then heat the system to 80°C, continue stirring and react for 4 hours, then add deionized water to carry out hydrolysis reaction for 3 hours. After the reaction is completed, cool down to obtain a phosphate compound;
[0073] S2: 9.34 g of methyltrimethoxysilane, 8.64 g of dimethyldimethoxysilane, 9.21 g of hexamethyldisilane and 38 mL of anhydrous ethanol are added to a container equipped with a reflux condenser, a thermometer and a dropping funnel, the mixed liquid is stirred, heated to 60°C, 7 mL of deionized water is added for hydrolysis reaction, and hydrochloric acid is added dropwise. After the addition is completed, the reaction is heated at a constant temperature for 3 hours, and 20 mL of butyl titanate dissolved in 30 mL of xylene is added dropwise. After the addition is completed, 3 mL of deionized water is added, hydrolysis is carried out for 4 hours, and vacuum distillation is carried out. The temperature is raised to 130°C for condensation for 2 hours to obtain a titanium-containing compound;
[0074] S3: 27.52 g of neopentyl glycol, 8.14 g of trimethylolpropane and 27.45 g of diethylene glycol were added to a container containing a thermometer, a reflux condenser, a water separator and a stirrer, and after nitrogen was introduced, the temperature was raised to 140° C. and stirred for 40 min, and then 48.71 g of isophthalic acid, 20 mL of xylene and dibutyltin dilaurate were added, and the temperature was raised to 180° C. for reaction for 5 h, and then the temperature was continued to be raised to 220° C. for reaction for 6 h. After the reaction was completed, the temperature was lowered to 160° C. and 11.22 g of sebacic acid was added, and the temperature was continued to be raised to 210° C. for reaction for 3 h. After the reaction was completed, the temperature was cooled, and 18 mL of xylene was added for dilution to obtain a polyester resin;
[0075] S4: Add 18 mL of phosphoric acid compound to 13 mL of polyester resin, heat to 85°C and stir to react for 2.5 hours, then add 9 mL of titanium-containing compound and dibutyltin dilaurate. After the addition is complete, heat to 170°C and react for 2 hours. After the reaction is completed, cool and discharge to obtain a modified resin.
[0076] This embodiment discloses a processing technology for a high temperature low alloy steel track shoe, comprising the following steps:
[0077] Step (1): 95.715 g Fe, 0.45 g Si, 1.55 g Mn, 0.85 g Cr, 1.15 g Ni, 0.25 g Mo and 0.035 g microcrystalline carbide are ball-milled, wherein the ball-milling medium is stainless steel balls, the ball-milling time is 23 h, and the ball-milling speed is 400 rpm, to obtain a low alloy mixture;
[0078] Step (2): heating the low alloy mixture to 900°C for normalizing, heating to 920°C for quenching, high temperature tempering at 650°C, surface quenching at 900°C and low temperature tempering at 200°C to obtain a low alloy crude product;
[0079] Step (3): 20 mL of the modified resin and 2 mL of the polyisocyanate curing agent are stirred and mixed for 30 minutes, and then coated on the surface of the low-alloy crude product. The surface of the low-alloy crude product is first cleaned with acetone and ethanol, and then coated after drying. The product is cured at 180° C. for 15 minutes to obtain a high-temperature low-alloy steel track shoe. Example 3
[0080] This embodiment discloses a method for preparing microcrystalline carbide, comprising the following steps:
[0081] Q1: 1.22g carbon powder and 9.47g niobium powder were fully ground in a mortar to make them uniform and of similar particle size. The mixed material was placed in a tablet press for tableting at 150MPa for 5min to obtain a thin disc;
[0082] Q2: Put the graphite pot with thin discs into a water-cooled copper pot, use tungsten rod as cathode material, and fix the graphite pot as anode material in a DC arc instrument, seal it with a columnar glass cover, start the power supply, turn on the vacuum pump to evacuate the air in the glass cover, when the air pressure is less than 10Pa, temporarily turn off the vacuum pump, slowly pass 40kPa of nitrogen, and evacuate again. After the evacuation is completed, fill in 40kPa of nitrogen, start the water-cooled circulation system, turn on the DC arc welder, adjust the current of the arc welder to 100A, react for 10 minutes after the arc is generated, and when the reaction is over, turn off the power supply and passivate for 4 hours in a nitrogen atmosphere. After passivation, collect the substances on the graphite pot to obtain microcrystalline carbide.
[0083] This embodiment discloses a method for preparing a modified resin, comprising the following steps:
[0084] S1: Add 2.15 mL of anhydrous ethanol and 1.00 g of phosphorus pentoxide to a container under ice water bath conditions, stir and mix evenly, then heat the system to 80°C, continue stirring and react for 4 hours, then add deionized water to carry out hydrolysis reaction for 3 hours. After the reaction is completed, cool down to obtain a phosphate compound;
[0085] S2: 9.76 g of methyltrimethoxysilane, 8.78 g of dimethyldimethoxysilane, 9.35 g of hexamethyldisilane and 42 mL of anhydrous ethanol are added to a container equipped with a reflux condenser, a thermometer and a dropping funnel, the mixed liquid is stirred, heated to 60°C, 10 mL of deionized water is added for hydrolysis reaction, and hydrochloric acid is added dropwise. After the addition is completed, the reaction is heated at a constant temperature for 3 hours, and 24 mL of butyl titanate dissolved in 35 mL of xylene is added dropwise. After the addition is completed, 3 mL of deionized water is added, hydrolysis is carried out for 4 hours, and vacuum distillation is carried out. The temperature is raised to 130°C for condensation for 2 hours to obtain a titanium-containing compound;
[0086] S3: 27.92 g of neopentyl glycol, 8.42 g of trimethylolpropane and 28.23 g of diethylene glycol were added to a container containing a thermometer, a reflux condenser, a water separator and a stirrer, and after nitrogen was introduced, the temperature was raised to 140° C. and stirred for 40 min, and then 49.01 g of isophthalic acid, 20 mL of xylene and dibutyltin dilaurate were added, and the temperature was raised to 180° C. for reaction for 5 h, and then the temperature was continued to be raised to 220° C. for reaction for 6 h. After the reaction was completed, the temperature was lowered to 160° C. and 11.44 g of sebacic acid was added, and the temperature was continued to be raised to 210° C. for reaction for 3 h. After the reaction was completed, the temperature was cooled, and 18 mL of xylene was added for dilution to obtain a polyester resin;
[0087] S4: Add 22 mL of phosphoric acid compound to 15 mL of polyester resin, heat to 85°C and stir to react for 2.5 hours, then add 13 mL of titanium-containing compound and dibutyltin dilaurate. After the addition is complete, heat to 170°C and react for 2 hours. After the reaction is completed, cool and discharge to obtain a modified resin.
[0088] This embodiment discloses a processing technology for a high temperature low alloy steel track shoe, comprising the following steps:
[0089] Step (1): 95.675 g Fe, 0.85 g Si, 1.15 g Mn, 1.05 g Cr, 0.75 g Ni, 0.45 g Mo and 0.075 g microcrystalline carbide are ball-milled and mixed, wherein the ball-milling medium is stainless steel balls, the ball-milling time is 23 h, and the ball-milling speed is 400 rpm, to obtain a low alloy mixture;
[0090] Step (2): heating the low alloy mixture to 900°C for normalizing, heating to 920°C for quenching, high temperature tempering at 650°C, surface quenching at 900°C and low temperature tempering at 200°C to obtain a low alloy crude product;
[0091] Step (3): 30 mL of the modified resin and 5 mL of the polyisocyanate curing agent are stirred and mixed for 30 minutes, and then coated on the surface of the low-alloy crude product. The surface of the low-alloy crude product is first cleaned with acetone and ethanol, and then coated after drying. The product is cured at 180° C. for 15 minutes to obtain a high-temperature low-alloy steel track shoe. Example 4
[0092] This embodiment discloses a method for preparing microcrystalline carbide, comprising the following steps:
[0093] Q1: 1.08g carbon powder and 8.32g niobium powder were fully ground in a mortar to make them uniform and of similar particle size. The mixed material was placed in a tablet press for tableting at 150MPa for 5min to obtain a thin disc;
[0094] Q2: Put the graphite pot with thin discs into a water-cooled copper pot, use tungsten rod as cathode material, and fix the graphite pot as anode material in a DC arc instrument, seal it with a columnar glass cover, start the power supply, turn on the vacuum pump to evacuate the air in the glass cover, when the air pressure is less than 10Pa, temporarily turn off the vacuum pump, slowly pass 40kPa of nitrogen, and evacuate again. After the evacuation is completed, fill in 40kPa of nitrogen, start the water-cooled circulation system, turn on the DC arc welder, adjust the current of the arc welder to 100A, react for 10 minutes after the arc is generated, and when the reaction is over, turn off the power supply and passivate for 4 hours in a nitrogen atmosphere. After passivation, collect the substances on the graphite pot to obtain microcrystalline carbide.
[0095] This embodiment discloses a method for preparing a modified resin, comprising the following steps:
[0096] S1: Add 2.02 mL of anhydrous ethanol and 1.073 g of phosphorus pentoxide to a container under ice water bath conditions, stir and mix evenly, then heat the system to 80°C, continue stirring and react for 4 hours, then add deionized water to carry out hydrolysis reaction for 3 hours. After the reaction is completed, cool down to obtain a phosphate compound;
[0097] S2: 9.42 g of methyltrimethoxysilane, 8.67 g of dimethyldimethoxysilane, 9.25 g of hexamethyldisilane and 41 mL of anhydrous ethanol are added to a container equipped with a reflux condenser, a thermometer and a dropping funnel, the mixed liquid is stirred, heated to 60°C, 8 mL of deionized water is added for hydrolysis reaction, and hydrochloric acid is added dropwise. After the addition is completed, the reaction is heated at a constant temperature for 3 hours, and 23 mL of butyl titanate dissolved in 31 mL of xylene is added dropwise. After the addition is completed, 3 mL of deionized water is added, hydrolysis is carried out for 4 hours, and vacuum distillation is carried out. The temperature is raised to 130°C for condensation for 2 hours to obtain a titanium-containing compound;
[0098] S3: 27.58 g of neopentyl glycol, 8.16 g of trimethylolpropane and 27.62 g of diethylene glycol were added to a container containing a thermometer, a reflux condenser, a water separator and a stirrer, and after nitrogen was introduced, the temperature was raised to 140° C. and stirred for 40 min, and then 48.78 g of isophthalic acid, 20 mL of xylene and dibutyltin dilaurate were added, and the temperature was raised to 180° C. for reaction for 5 h, and then the temperature was continued to be raised to 220° C. for reaction for 6 h. After the reaction was completed, the temperature was lowered to 160° C. and 11.28 g of sebacic acid was added, and the temperature was continued to be raised to 210° C. for reaction for 3 h. After the reaction was completed, the temperature was cooled, and 18 mL of xylene was added for dilution to obtain a polyester resin;
[0099] S4: Add 19 mL of phosphoric acid compound to 14.5 mL of polyester resin, heat to 85°C and stir to react for 2.5 hours, then add 12 mL of titanium-containing compound and dibutyltin dilaurate. After the addition is complete, heat to 170°C and react for 2 hours. After the reaction is completed, cool and discharge to obtain a modified resin.
[0100] This embodiment discloses a processing technology for a high temperature low alloy steel track shoe, comprising the following steps:
[0101] Step (1): 96.18 g Fe, 0.48 g Si, 1.17 g Mn, 0.88 g Cr, 0.80 g Ni, 0.42 g Mo and 0.07 g microcrystalline carbide are ball-milled and mixed, wherein the ball-milling medium is stainless steel balls, the ball-milling time is 23 h, and the ball-milling speed is 400 rpm, to obtain a low alloy mixture;
[0102] Step (2): heating the low alloy mixture to 900°C for normalizing, heating to 920°C for quenching, high temperature tempering at 650°C, surface quenching at 900°C and low temperature tempering at 200°C to obtain a low alloy crude product;
[0103] Step (3): 28 mL of the modified resin and 4 mL of the polyisocyanate curing agent were stirred and mixed for 30 minutes, and then coated on the surface of the low-alloy crude product. The surface of the low-alloy crude product was first cleaned with acetone and ethanol, and then coated after drying. The product was cured at 180° C. for 15 minutes to obtain a high-temperature low-alloy steel track shoe.
[0104] Comparative Example 1
[0105] Comparative Example 1 Compared with Example 1, in the process of preparing microcrystalline carbide in Comparative Example 1, no carbon powder is added, and other conditions remain unchanged.
[0106] Comparative Example 2
[0107] Comparative Example 2 Compared with Example 1, in the process of preparing microcrystalline carbide in Comparative Example 2, no niobium powder is added, and other conditions remain unchanged.
[0108] Comparative Example 3
[0109] Comparative Example 3 Compared with Example 1, in the process of preparing the modified resin in Comparative Example 3, phosphorus pentoxide was not added, and other conditions remained unchanged.
[0110] Comparative Example 4
[0111] Comparative Example 4 Compared with Example 1, in the process of preparing the modified resin in Comparative Example 4, methyltrimethoxysilane was not added, and other conditions remained unchanged.
[0112] Comparative Example 5
[0113] Comparative Example 5 Compared with Example 1, in the process of preparing the modified resin in Comparative Example 5, no butyl titanate was added, and other conditions remained unchanged.
[0114] Comparative Example 6
[0115] Comparative Example 6 Compared with Example 1, in the process of preparing the modified resin in Comparative Example 6, no neopentyl glycol was added, and other conditions remained unchanged.
[0116] Comparative Example 7
[0117] Compared with Example 1, in Comparative Example 7, during the preparation of the high-temperature low-alloy steel track shoe, no microcrystalline carbide is added, and other conditions remain unchanged.
[0118] Comparative Example 8
[0119] Compared with Example 1, in Comparative Example 8, during the preparation of the high-temperature low-alloy steel track shoe, no modified resin was added, and other conditions remained unchanged.
[0120] The performance of the high temperature low alloy steel track shoes prepared in Examples 1-4 and Comparative Examples 1-8 was tested. The hardness of the samples was tested according to GB / T231.1-2018, the wear resistance of the samples was tested according to GB / T 12444.2-2006, the high temperature resistance of the samples was tested according to GB / T 4338-2006, and the corrosion resistance of the samples was tested according to GB / T 10125-2012. The test results are shown in Table 1:
[0121] Table 1
[0122]
[0123] It can be seen from the test results in Table 1 that the high-temperature low-alloy steel track shoes prepared in Examples 1-4 of the present invention have excellent wear resistance, high temperature resistance, corrosion resistance and high hardness. Comparison between Comparative Example 1 and Examples 1-4 shows that the addition of carbon powder can effectively improve the hardness, wear resistance and high temperature resistance of the high-temperature low-alloy steel track shoes; comparison between Comparative Example 2 and Examples 1-4 shows that the addition of niobium powder can effectively improve the hardness, wear resistance and high temperature resistance of the high-temperature low-alloy steel track shoes; comparison between Comparative Example 3 and Examples 1-4 shows that the addition of phosphorus pentoxide can effectively improve the corrosion resistance of the high-temperature low-alloy steel track shoes; comparison between Comparative Example 4 and Examples 1-4 shows that the addition of methyltrimethoxysilane can effectively improve the corrosion resistance of the high-temperature low-alloy steel track shoes. Corrosion performance; by comparing comparative example 5 with embodiments 1-4, it can be seen that the addition of butyl titanate can effectively improve the corrosion resistance of the high-temperature low-alloy steel track shoe; by comparing comparative example 6 with embodiments 1-4, it can be seen that the addition of neopentyl glycol can effectively improve the corrosion resistance of the high-temperature low-alloy steel track shoe; by comparing comparative example 7 with embodiments 1-4, it can be seen that the addition of microcrystalline carbide can effectively improve the hardness, wear resistance and high temperature resistance of the high-temperature low-alloy steel track shoe; by comparing comparative example 8 with embodiments 1-4, it can be seen that the addition of modified resin can effectively improve the corrosion resistance of the high-temperature low-alloy steel track shoe.
[0124] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
[0125] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. The processing technology of high temperature low alloy steel track shoe is characterized by: The following steps are involved: Step (1): ball-milling and mixing Fe, Si, Mn, Cr, Ni, Mo and microcrystalline carbides to obtain a low alloy mixture; Step (2): subjecting the low alloy mixture to temperature normalizing, temperature quenching, high temperature tempering, surface quenching and low temperature tempering treatments to obtain a low alloy crude product; Step (3): stirring and mixing the modified resin and the polyisocyanate curing agent, applying the mixture to the surface of the low alloy crude product, and curing the mixture to obtain a high temperature low alloy steel track shoe; The method for preparing the microcrystalline carbide comprises the following steps: Q1: Grind carbon powder and niobium powder in a mortar until they are evenly mixed and have similar particle sizes. Place the mixed material in a tablet press for tableting to obtain thin discs. Q2: Put the graphite pot with the thin disc into the water-cooled copper pot, use the tungsten rod as the cathode material, fix the graphite pot as the anode material in the DC arc instrument, seal it with a columnar glass cover, start the power supply, turn off the power supply after the reaction is completed, passivate in a nitrogen atmosphere, collect the material on the graphite pot after passivation, and obtain microcrystalline carbide; The preparation method of the modified resin comprises the following steps: S1: adding anhydrous ethanol and phosphorus pentoxide to a container under ice water bath conditions, stirring and mixing evenly, heating the system, and continuing to stir and react, then adding deionized water for hydrolysis reaction, and after the reaction is completed, cooling to obtain a phosphate compound; S2: Add methyltrimethoxysilane, dimethyldimethoxysilane, hexamethyldisilane and anhydrous ethanol into a container equipped with a reflux condenser, a thermometer and a dropping funnel, stir the mixed liquid, heat and raise the temperature, add deionized water for hydrolysis reaction, and dropwise add hydrochloric acid. After the dropwise addition is completed, heat and react at a constant temperature, then dropwise add butyl titanate dissolved in xylene, add deionized water after the dropwise addition is completed, hydrolyze, distill under reduced pressure, and heat and condense to obtain a titanium-containing compound; S3: adding neopentyl glycol, trimethylolpropane and diethylene glycol to a container containing a thermometer, a reflux condenser, a water separator and a stirrer, introducing nitrogen, heating and stirring, then adding isophthalic acid, xylene and dibutyltin dilaurate, heating to react, then continuing to heat to react, after the reaction is completed, cooling and adding sebacic acid, continuing to heat to react, after the reaction is completed, cooling, adding xylene to dilute, and obtaining a polyester resin; S4: adding a phosphoric acid compound to the polyester resin, heating and stirring to react, then adding a titanium-containing compound and dibutyltin dilaurate, after the addition is complete, heating to react, after the reaction is completed, cooling and discharging to obtain a modified resin.
2. The processing technology of high temperature low alloy steel track shoe according to claim 1 is characterized in that: In the step (1), the mass ratio of Fe, Si, Mn, Cr, Ni, Mo and microcrystalline carbide is (95.55-96.45): (0.45-0.85): (1.15-1.55): (0.85-1.05): (0.75-1.15): (0.25-0.45): (0.035-0.075). During the ball milling mixing process, the ball milling medium is stainless steel balls, the ball milling time is 20-30 hours, and the ball milling speed is 300-400 rpm.
3. The processing technology of high temperature low alloy steel track shoe according to claim 1 is characterized in that: In the Q1, the molar ratio of carbon powder to niobium powder is (0.9-1.1): (0.9-1.1). During the tableting process, the applied pressure is 150-170MPa for 3-5min. In the Q2, after starting the power supply, the vacuum pump is turned on to evacuate the air in the glass cover. When the air pressure is less than 10Pa, the vacuum pump is temporarily turned off, and 30-50kPa of nitrogen is slowly introduced, and the air is evacuated again. After the evacuation is completed, 40kPa of nitrogen is filled, the water cooling circulation system is started, the DC arc welding machine is turned on, the current of the arc welding machine is adjusted to 100A, and the reaction is carried out for 8-10min after the arc is generated. The reaction is completed and the passivation time is 3-4h.
4. The processing technology of high temperature low alloy steel track shoe according to claim 1, characterized in that: In the step (2), the temperature of the normalizing is 800-950°C, the temperature of the quenching is 850-920°C, the temperature of the high temperature tempering is 550-650°C, the temperature of the surface quenching is 850-900°C, and the temperature of the low temperature tempering is 150-200°C.
5. The processing technology of high temperature low alloy steel track shoe according to claim 1, characterized in that: In the S1, the molar ratio of anhydrous ethanol and phosphorus pentoxide is (3.8-4.2): (0.8-1.1), the heating temperature is 75-80°C, the stirring reaction time is 3-4h, and the hydrolysis reaction time is 2-3h; in the S2, the amount ratio of methyltrimethoxysilane, dimethyldimethoxysilane, hexamethyldisilane, anhydrous ethanol, deionized water, xylene and butyl titanate is (9.34-9.76) g: (8.64-8.78) g: (9.21-9.35) g: (38-42) mL: (7-10) mL: (30-35) mL: (20-24) mL, the heating temperature is 60-70°C, the constant temperature heating reaction time is 2-3h, the hydrolysis time is 3-4h, the heating condensation temperature is 120-130°C, and the time is 2-3h.
6. The processing technology of high temperature low alloy steel track shoe according to claim 1, characterized in that: In the S3, the mass ratio of neopentyl glycol, trimethylolpropane, diethylene glycol, isophthalic acid and sebacic acid is (27.52-27.92) g: (8.14-8.42) g: (27.45-28.23) g: (48.71-49.01) g: (11.22-11.44) g, the heating stirring temperature is 130-140°C, the time is 30-40 min, the heating reaction temperature is 170-180°C, the time is 4-5 h, and the reaction is continued. The heating reaction temperature is 210-220°C, the time is 6-8h, the cooling temperature is 160-170°C, and the heating temperature is continued to be 200-210°C, and the time is 2-3h; in the S4, the volume ratio of the phosphoric acid compound, the polyester resin and the titanium-containing compound is (18-22) mL: (13-15) mL: (9-13) mL, the heating and stirring reaction temperature is 75-85°C, the time is 2-2.5h, and the heating reaction temperature is 170-180°C, and the time is 1-2h.
7. The processing technology of high temperature low alloy steel track shoe according to claim 1, characterized in that: In the step (3), the ratio of the modified resin to the polyisocyanate curing agent is (20-30) mL: (2-5) mL, the stirring mixing time is 20-30 min, the surface of the crude low alloy product is first cleaned with acetone and ethanol, and then coated after drying, the curing temperature is 150-180°C, and the time is 10-15 min.
Citation Information
Patent Citations
Manufacturing methods of high-strength steel and high-strength steel track plates
CN112813362B
Low alloy steel used for making track board of crawling crane and preparation method thereof
CN101876030A
Low-alloy ultrahigh-strength wear-resistant steel and production method thereof
CN102605272A
Segmented hardness low-alloy steel hammer head and manufacturing method thereof
CN102676946A
Multi-element low-alloy abrasion-resistant cast steel containing nanocrystalline austenite and preparation method thereof
CN109440001A