Single crystal positive electrode material and preparation method thereof, and lithium ion battery

By controlling the particle size and particle size distribution of nickel-cobalt-manganese positive electrode material, combined with the core-shell structure and multi-step sintering process, the problems of fragility and poor safety performance of single-crystal positive electrode material are solved, and the compaction density and circulation of the battery are improved. Performance ensures safety performance at high nickel content.

CN118486814BActive Publication Date: 2024-11-08NINGBO RONBAY LITHIUM BATTERY MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410939416.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-08
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

The existing single crystal positive electrode materials are fragile during electrode preparation, have low compaction density, which affects the charging/discharging performance and cycle stability of the battery. The safety performance of high nickel materials is poor, which easily leads to thermal runaway.

Method used

Using nickel-cobalt-manganese as the ternary positive electrode material, a single peak distribution is formed by controlling the particle size and particle size distribution, enhancing the particle strength, and a core-shell structure is designed on the structure, doping elements M and N to improve diffusion rate and surface stability. , combined with a multi-step sintering process to improve the compaction density and safety performance of the material.

Benefits of technology

The compaction density and cycling performance of the cathode material are improved, the safety performance and energy density of the battery are enhanced, the thermal stability and chemical stability problems are avoided, and the safety performance under high nickel content is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118486814B_ABST
    Figure CN118486814B_ABST
Patent Text Reader

Abstract

The present invention provides a single crystal positive electrode material and a preparation method thereof, and a lithium ion battery. When the positive electrode material is subjected to a pressure of 8T-10T, its particle size volume distribution is a single peak distribution. The present invention provides a positive electrode material with nickel, cobalt and manganese as ternary. The particle size and particle size distribution of the positive electrode material have a certain influence on the safety performance of the battery, the compaction density of the pole piece, and the cycle performance of the battery. When the positive electrode material is subjected to a pressure of 8T-10T, the particle size volume distribution of the positive electrode material can be represented by a particle size differential distribution curve, and the detection shows that the particle size volume distribution of the positive electrode material provided by the present invention is a single peak distribution from beginning to end during the process of being subjected to pressure, indicating that the particle strength of the positive electrode material is high and has strong structural stability, which ensures that the positive electrode material is not damaged or broken under a large pressure, and further, it has an important positive impact on battery performance, cycle life, safety and energy density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a single crystal positive electrode material and a preparation method thereof, and a lithium ion battery. Background Art

[0002] With the widespread popularity of new energy electric vehicles and the frequent occurrence of spontaneous combustion of new energy vehicles in recent years, people's focus has gradually shifted from driving range to safety performance. As one of the main materials of lithium-ion batteries, cathode materials have been greatly challenged, among which the most prominent is ternary cathode materials. As the nickel content of ternary cathode materials increases, the capacity gradually increases, but the stability of the material gradually decreases.

[0003] In the prior art, there are some problems with single crystal positive electrode materials as positive electrode materials for lithium-ion batteries: single crystal positive electrode materials usually have high hardness and brittleness, which makes them prone to fragmentation or breakage during the preparation of the electrode, especially in the mixing, compaction and molding stages of the preparation process. Brittleness may cause material fragmentation and reduce the stability of the electrode. Since the particle structure of single crystal materials is large and irregular in shape, it is difficult to achieve high-density compaction of single crystal materials in electrode preparation, which will affect the charge / discharge performance and cycle stability of the electrode. Single crystal positive electrode materials usually have a high pyrolysis temperature, that is, they are prone to thermal decomposition or structural damage at high temperatures, which will limit the operating temperature range and thermal stability of the battery.

[0004] In order to solve the above problems, a common practice is to mix single crystal cathode materials with polycrystalline materials, thereby solving the problems of poor compaction performance and mechanical stability, high pyrolysis temperature, etc. of single crystal cathode materials. However, it also faces many limitations and problems such as electrochemical performance optimization, increased material costs, and challenges in process control. Therefore, there is an urgent need for a single crystal ternary cathode material with high capacity, higher compaction density and cycle performance, so as to improve the competitiveness of single crystal ternary cathode materials. Summary of the invention

[0005] The present invention aims to solve the problems in the prior art that high nickel single crystal positive electrode materials have low compaction density, insufficient energy density, poor safety performance, and need to be mixed with polycrystalline materials for use as positive electrode materials.

[0006] In order to solve the above problems, the present invention provides a single crystal positive electrode material. When the positive electrode material is subjected to a pressure of 8T-10T, the particle size volume distribution of the positive electrode material is a single peak distribution.

[0007] The present invention provides a positive electrode material with nickel, cobalt and manganese as ternary materials. The particle size and particle size distribution of the positive electrode material have a great influence on the safety performance of the battery and the compaction density of the pole piece, and also have a certain influence on the cycle performance of the battery. When the positive electrode material is subjected to a pressure of 8T-10T, the particle size volume distribution of the positive electrode material can be represented by a particle size differential distribution curve. The test shows that the particle size volume distribution of the positive electrode material provided by the present invention is a single-peak distribution from beginning to end during the process of being subjected to pressure, indicating that the particle strength of the positive electrode material is relatively high and has strong structural stability, thereby ensuring that the positive electrode material can withstand greater pressure without being damaged or broken, and further, it has an important positive impact on battery performance, cycle life, safety and energy density.

[0008] The positive electrode material of the present invention has a single crystal particle shape, and the particle size is controlled within a relatively high range, thereby avoiding the grain boundary cracking caused during the battery charging and discharging process, and ensuring the excellent cycle performance of the battery. In addition, the single crystal particles can also increase the compaction density of the positive electrode material, thereby increasing the energy density.

[0009] In any of the above technical solutions, under the condition that the positive electrode material is subjected to a pressure of 8T-10T, the particle size D50 of the positive electrode material before being subjected to the pressure is 1 Particle size after pressure D50 2 The numerical range of the change difference △D50 is 0μm<△D50<0.1μm; among them, the particle size D50 of the positive electrode material before being subjected to pressure 1 The size range is 4μm<D50 1 <7μm.

[0010] When the positive electrode material is subjected to a pressure of 8T-10T, the numerical range of the difference △D between the particle size before and after the pressure is △D50<0.1μm, indicating that the positive electrode material does not produce obvious particle size changes after being subjected to a large pressure, thereby ensuring that the positive electrode material has a high compaction density and excellent cycle performance, avoiding serious safety problems caused by poor thermal stability and chemical stability under deep charge and discharge conditions.

[0011] The particle size range of the positive electrode material before being subjected to pressure is controlled to 4μm<D50 1<7μm, the particle size range is the median particle size range, the particle size of the positive electrode material provided by the present invention is relatively large, the larger the particle size, the better the dispersibility of the single crystal positive electrode material, the higher the tap density, and the greater the compaction density of the pole piece prepared from the positive electrode material, thereby ensuring that the strength of the positive electrode material is high, so that it can withstand greater pressure without breaking. A higher compaction density ensures that the positive electrode material has a higher energy density, thereby ensuring higher safety performance of the battery.

[0012] In any of the above technical solutions, the compaction density PD of the positive electrode material powder is in the range of PD ≥ 3.7 g / cm 3 ; and / or the compaction density CD of the electrode sheet prepared from the positive electrode material has a value range of CD ≥ 3.55 g / cm 3 .

[0013] The compaction density PD of the cathode material powder is in the range of PD ≥ 3.7 g / cm 3 ; and / or the compaction density CD of the electrode sheet prepared from the positive electrode material has a value range of CD ≥ 3.55 g / cm 3 , indicating that the powder of the positive electrode material provided by the present invention and the prepared electrode sheet have a higher compaction density. Appropriate compaction density can increase the discharge capacity of the battery, thereby improving the utilization rate of the lithium-ion battery.

[0014] In any of the above technical solutions, when the nickel content of the positive electrode material is 50%-80%, the peak thermal decomposition temperature at a charge cut-off voltage of 4.45V is not less than 250°C; and / or when the nickel content of the positive electrode material is greater than 80%, the peak thermal decomposition temperature at a charge cut-off voltage of 4.3V is not less than 225°C.

[0015] During the charging and discharging process of high-nickel batteries, the charged positive electrode will release heat, which will trigger a thermal decomposition reaction, resulting in thermal runaway of the battery, which will lead to poor safety performance of the high-nickel positive electrode material; the greater the voltage of the battery, the greater the amount of lithium removed from the positive electrode material, which will lead to poor safety performance of the positive electrode material. The positive electrode material provided in this embodiment has a higher compaction density, and while ensuring a higher nickel content, it has better safety performance and a higher thermal decomposition peak temperature even under high pressure.

[0016] In any of the above technical solutions, the positive electrode material includes a core layer and a shell layer, the shell layer is coated on at least part of the surface of the core layer, and the thickness of the shell layer is in the range of 10nm-20nm; the composition of the positive electrode material is shown in formula (I):

[0017] Li m [Ni x Co y Mn z Ma N b ]O 2 (I);

[0018] In the positive electrode material, the value ranges of m, x, y, z, a, and b are as follows: 0.98<m<1.05, 0.5<x<1, 0<y<0.2, 0<z<0.2, 0<a<0.1, x+y+z+a+b=1; wherein, element M is doped in the core layer, and element M includes at least one of Al, Ga, Mg, La, Y, Zn, V, and Sr; element N is doped in the shell layer, and element N includes at least one of Ti, Zr, Nb, Mo, Ta, W, and Ce.

[0019] The present invention provides a cathode material with nickel, cobalt and manganese as ternary elements, wherein the structure includes a core layer and a shell layer, and the core-shell structure can not only improve the stability of the overall structure of the cathode material and the diffusion rate of lithium ions, but also improve the stability of the surface structure of the cathode material; the cathode material is doped with element M and element N, wherein the diffusion rate of element M in the cathode material is greater than the diffusion rate of element N in the cathode material, and according to the diffusion rate of the doped element, it is ensured that element M is doped in the core layer and element N is doped in the shell layer.

[0020] The shell layer of the positive electrode material is wrapped around at least part of the surface of the core layer of the positive electrode material, and the shell layer is doped with element N. The doping of element N can effectively improve the stability of the surface structure of the positive electrode material, wherein the thickness range of the shell layer is controlled between 10nm-20nm, and the setting of this thickness is more conducive to the diffusion of lithium ions.

[0021] The diffusion rate of element M in the positive electrode material is greater than the diffusion rate of element N in the positive electrode material. Element M diffuses relatively quickly in the positive electrode material, and is mainly evenly distributed in the core layer of the positive electrode material; element N diffuses relatively slowly in the positive electrode material, and is mainly doped in the shallow layer of the positive electrode material to form a shell structure, which is mainly used to improve the shallow layer stability of the material. The positive electrode material with a core-shell structure obtained by doping elements M and N has the characteristics of high strength, ability to withstand high voltage, and good safety performance. Among them, by doping element M in the core layer, the stability of the overall structure of the positive electrode material and the diffusion rate of lithium ions can be improved, and by doping element N in the shell layer, the stability of the surface structure of the positive electrode material can be improved.

[0022] In any of the above technical solutions, when the nickel content of the positive electrode material is 50%-80%, the tap density TD of the positive electrode material is ≥2.5g / cm 3 ; and / or when the nickel content of the positive electrode material is 80%-90%, the tap density TD of the positive electrode material is ≥2.3g / cm 3; and / or when the nickel content of the positive electrode material is 90%-100%, the tap density of the positive electrode material TD ≥ 2.1g / cm 3 .

[0023] The value range of nickel content in the positive electrode material is 0.5<x<1. The value range of nickel content in the present invention can ensure that the positive electrode material has a higher tap density. At this time, if the positive electrode material also has a higher strength, the prepared positive electrode sheet has a higher compaction density, thereby increasing the energy density of the battery. Among them, the higher the nickel content, the more difficult it is for single crystal particles to grow during sintering of the material, making the morphology of the positive electrode material difficult to control, which leads to a lower tap density; in addition, the higher the nickel content of the positive electrode material, the lower the lithium-nickel mixing ratio, which can improve the stability of the battery cycle, but at this time the tap density of the positive electrode material is also lower, and the energy density of the battery is also smaller. Therefore, it is necessary to select a suitable range of nickel content to ensure that the battery has good cycle performance and a higher energy density.

[0024] In any of the above technical solutions, the value range of the lithium-nickel mixing ratio Li / Ni mixing of the positive electrode material is 0%<Li / Ni mixing<2%.

[0025] A higher sintering temperature is required in the process of preparing positive electrode materials with single crystal morphology, but high temperature can easily cause lithium-nickel mixing. A higher lithium-nickel mixing ratio can not only easily lead to the aggravation of interfacial side reactions, but also reduce the capacity of the battery. Therefore, the lithium-nickel mixing ratio Li / Ni mixing of the positive electrode material is controlled in the range of 0%<Li / Ni mixing<2%. A lower lithium-nickel mixing ratio can effectively improve the stability of the crystal structure, thereby improving the cycle stability of the positive electrode material.

[0026] The present invention also provides a method for preparing a single crystal positive electrode material, the method for preparing the positive electrode material as described above, the method comprising the following steps: primary sintering: sintering a Li source, a Ni / Co / Mn ternary precursor, and an oxide containing element M to obtain a sintered product; secondary sintering: sintering the sintered product and a compound containing element N to obtain a positive electrode material; wherein the temperature curve of the primary sintering sequentially comprises a first temperature section T 1 , the second temperature section T 2 , the third temperature section T 3 And the fourth temperature section T 4 ; T 1 、T 2 、T 3 、T 4 The value ranges of T are as follows: 1 400℃-600℃; T 1 <T 2 ≤800℃; T2 +100℃<T 3 ≤1000℃;T 1 <T 4 ≤800℃; first temperature section T 1 , the second temperature section T 2 , the fourth temperature section T 4 The oxygen flux is greater than the third temperature section T 3 oxygen flux; element M includes at least one of Al, Ga, Mg, La, Y, Zn, V, and Sr; element N includes at least one of Ti, Zr, Nb, Mo, Ta, W, and Ce.

[0027] The preparation method for preparing positive electrode materials provided by the present invention is to prepare the required positive electrode materials by performing primary sintering and secondary sintering. Among them, the Li source, the Ni / Co / Mn ternary precursor, and the oxide containing the M element are sintered once, and then the sintered product and the compound of the N element are sintered twice to finally prepare the positive electrode material. The diffusion rate of the element M in the ternary material is greater than that of the element N. According to the speed of the diffusion rate of the doping element in the ternary positive electrode material, step-by-step doping is performed, wherein the primary sintering is doped with the element with a high diffusion rate in the positive electrode material under high temperature conditions, and the secondary sintering is doped with the element with a slow diffusion rate in the positive electrode material under low temperature conditions to form a core-shell structure with good safety performance. The positive electrode material with a core-shell structure obtained by combining a multi-step sintering process with doping elements has the characteristics of high strength, ability to withstand high voltage, and good safety performance.

[0028] A positive electrode material with a large single crystal size can be prepared under high temperature conditions. By setting different temperature sections, the lithium-nickel mixing and grain boundary phenomena caused by high temperature can be reduced. The overall lithium-nickel mixing degree of the positive electrode material is low, the dispersion degree is high, and it has a high compaction density and electrochemical performance. The element M with a faster diffusion rate is doped in the primary sintering process to make it evenly distributed in the material body. By setting four sintering temperature sections in the primary sintering step and limiting the sintering temperature, a single crystal positive electrode material with high strength is formed.

[0029] Among them, the second temperature section T 2 The role of is to form a layered and rock salt composite phase, which is more conducive to the formation of single crystals, reduce the generation of grain boundaries, and increase the dispersion of single crystals; the third temperature section T 3 The role of is to reduce the time and ventilation volume of the high temperature section, and to reduce the degree of lithium-nickel mixing. Among them, the temperature value of this temperature section is the highest, and its purpose is to promote more uniform growth of single crystals, and reducing the ventilation volume is to reduce oxidation during the growth process; the fourth temperature section T 4The function is to relieve the stress in the high temperature section and rearrange it, thereby increasing the strength of the positive electrode material.

[0030] By limiting the size of the oxygen flux during the sintering process, it is beneficial to form a single crystal positive electrode material with high strength, wherein in the third temperature section T of the primary sintering 3 The oxygen flux needs to be reduced to ensure the first temperature section T 1 , the second temperature section T 2 , the fourth temperature section T 4 The oxygen flux is greater than the third temperature section T 3 The oxygen flux is reduced, which helps to reduce the oxidation of the single crystal during the growth process.

[0031] In any of the above technical solutions, the first temperature section T 1 The maintenance time is 2h-8h; and / or the second temperature section T 2 The maintenance time is 2h-8h; and / or the third temperature section T 3 The maintenance time is 2h-6h; and / or the fourth temperature section T 4 The holding time is 2h-8h; and / or the heating rate of the first sintering is 1℃ / min-5℃ / min; and / or the heating rate of the second sintering is 1℃ / min-5℃ / min; and / or the sintering temperature of the second sintering is 700℃-900℃; and / or the sintering time of the second sintering is 8h-12h.

[0032] The process parameters of the maintenance time of the four sintering temperature sections in one sintering are related to the compaction density and strength of the positive electrode material. The selection of the maintenance time is to make the growth of the single crystal positive electrode material more uniform, the dispersion better, the strength higher, the internal stress distribution more uniform, and the electrochemical performance better. Therefore, this embodiment gives a preferred maintenance time range to obtain the positive electrode material claimed for protection in this application.

[0033] According to the diffusion rate of the doping elements in the positive electrode material, doping is carried out in steps, wherein the elements with high diffusion rate in the positive electrode material are doped under high temperature conditions in the first sintering, and the elements with slow diffusion rate in the positive electrode material are doped under low temperature conditions in the second sintering, forming a core-shell structure with good safety performance. The doping element M in the first sintering diffuses relatively quickly in the positive electrode material, and combined with the corresponding multi-stage sintering process, it is mainly evenly distributed in the core layer of the positive electrode material; the doping element N in the second sintering diffuses relatively slowly in the positive electrode material, and the sintering temperature is relatively low, and it is mainly doped in the shallow layer of the positive electrode material to form a shell structure, which is mainly used to improve the shallow surface stability of the material. The positive electrode material obtained by two-step sintering has the characteristics of high strength, ability to withstand high voltage, and good safety performance.

[0034] During the preparation of positive electrode materials, if the sintering heating rate is too fast, it will lead to uneven material growth and internal stress distribution, and if the heating rate is too slow, it will lead to a longer sintering cycle and increased energy consumption. Therefore, the present invention controls the heating rate of the first sintering at 1°C / min-5°C / min, and the heating rate of the secondary sintering at 1°C / min-5°C / min.

[0035] The present invention further provides a lithium ion battery, which includes the positive electrode material as described above. The lithium ion battery has the same beneficial effects as the positive electrode material as described above, so it will not be described in detail here.

[0036] After adopting the technical solution of the present invention, the following technical effects can be achieved:

[0037] (1) The single crystal size of the single crystal positive electrode material in the prior art is small (<2μm) and the compaction density is low. The single crystal positive electrode material provided by the present invention has a large size (D50 is 4μ-7μm), a high tap density, and a high electrode compaction density;

[0038] (2) The positive electrode material provided by the present invention has a core-shell structure, wherein the core layer contains an element with a high diffusion rate in the positive electrode material, and the shell layer contains an element with a low diffusion rate in the positive electrode material;

[0039] (3) The positive electrode material provided by the present invention has good safety performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0041] Figure 1 This is an electron microscope image of the positive electrode material provided in Example 1 of the present invention;

[0042] Figure 2 This is an EDS image of the cross section of the positive electrode material provided in Example 1 of the present invention;

[0043] Figure 3 This is an electron microscope image of the positive electrode material provided in Comparative Example 1 of the present invention;

[0044] Figure 4 This is an EDS image of the cross section of the positive electrode material provided in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0045] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] The embodiment of the present invention provides a single crystal positive electrode material. When the positive electrode material is subjected to a pressure of 8T-10T, the particle size volume distribution of the positive electrode material is a single peak distribution.

[0047] The present invention provides a positive electrode material with nickel, cobalt and manganese as ternary materials. The particle size and particle size distribution of the positive electrode material have a great influence on the safety performance of the battery and the compaction density of the pole piece, and also have a certain influence on the cycle performance of the battery. When the positive electrode material is subjected to a pressure of 8T-10T, the particle size volume distribution of the positive electrode material can be represented by a particle size differential distribution curve. The test shows that the particle size volume distribution of the positive electrode material provided by the present invention is a single-peak distribution from beginning to end during the process of being subjected to pressure, indicating that the particle strength of the positive electrode material is relatively high and has strong structural stability, thereby ensuring that the positive electrode material can withstand greater pressure without being damaged or broken, and further, it has an important positive impact on battery performance, cycle life, safety and energy density.

[0048] The technical means for improving the safety performance of positive electrode materials in the prior art include, on the one hand, doping and mixing single crystal materials with polycrystalline materials, and on the other hand, using single crystal materials with smaller sizes. However, these technical means all have the problem of low compaction density. Therefore, the morphology of the positive electrode material of the present invention is single crystal particles, and the particle size is controlled within a relatively high range, thereby avoiding the situation of grain boundary cracking caused by the battery charging and discharging process, and ensuring the excellent cycle performance of the battery. In addition, single crystal particles can also increase the compaction density of the positive electrode material, thereby increasing the energy density.

[0049] In some embodiments of the present application, when the positive electrode material is subjected to a pressure of 8T-10T, the particle size D50 of the positive electrode material before the pressure is applied is 1 Particle size after pressure D50 2 The numerical range of the change difference △D50 is 0μm<△D50<0.1μm; among them, the particle size D50 of the positive electrode material before being subjected to pressure 1 The range is 4μm<D50 1 <7μm.

[0050] When the positive electrode material is subjected to a pressure of 8T-10T, the numerical range of the change difference △D between the particle size of the positive electrode material before the pressure and the particle size after the pressure is △D50<0.1μm, indicating that the positive electrode material does not produce obvious changes in particle size after being subjected to a large pressure, thereby ensuring that the positive electrode material has a high compaction density and excellent cycle performance, and avoiding serious safety problems caused by poor thermal stability and chemical stability under deep charge and discharge conditions. Among them, the change difference △D50 is the particle size of the positive electrode material before the pressure minus the particle size after the pressure. Further preferably, under the condition that the positive electrode material is subjected to a pressure of 8T-10T, the numerical range of the change difference △D of the particle size of the positive electrode material is 0μm<△D50<0.06μm.

[0051] The particle size range of the positive electrode material before being subjected to pressure is controlled to 4μm<D50 1 <7μm, the particle size range is the median particle size range, the particle size of the positive electrode material provided by the present invention is relatively large, the larger the particle size, the better the dispersibility of the single crystal positive electrode material, the higher the tap density, and the greater the compaction density of the pole piece prepared from the positive electrode material, thereby ensuring that the strength of the positive electrode material is high, so that it can withstand greater pressure without breaking. A higher compaction density ensures that the positive electrode material has a higher energy density, thereby ensuring higher safety performance of the battery.

[0052] In some embodiments of the present application, the compaction density PD of the positive electrode material powder is in the range of PD ≥ 3.7 g / cm 3 ; and / or the compaction density CD of the electrode sheet prepared from the positive electrode material has a value range of CD ≥ 3.55 g / cm 3 .

[0053] The compaction density PD of the cathode material powder is in the range of PD ≥ 3.7 g / cm 3 ; and / or the compaction density CD of the electrode sheet prepared from the positive electrode material has a value range of CD ≥ 3.55 g / cm 3 , indicating that the powder of the positive electrode material provided by the present invention and the prepared electrode sheet have a higher compaction density. Appropriate compaction density can increase the discharge capacity of the battery, thereby improving the utilization rate of the lithium-ion battery.

[0054] In some embodiments of the present application, when the nickel content of the positive electrode material is 50%-80%, the peak thermal decomposition temperature at a charge cut-off voltage of 4.45V is not less than 250°C; and / or when the nickel content of the positive electrode material is greater than 80%, the peak thermal decomposition temperature at a charge cut-off voltage of 4.3V is not less than 225°C.

[0055] During the charging and discharging process of high-nickel batteries, the charged positive electrode will release heat, which will trigger a thermal decomposition reaction, resulting in thermal runaway of the battery, which will lead to poor safety performance of the high-nickel positive electrode material; the greater the voltage of the battery, the greater the amount of lithium removed from the positive electrode material, which will lead to poor safety performance of the positive electrode material. The positive electrode material provided in this embodiment has a higher compaction density, and has better safety performance while ensuring a higher nickel content. When the nickel content of the positive electrode material is 50%-80%, the peak temperature of thermal decomposition at a charging cut-off voltage of 4.45V is not less than 250°C; when the nickel content of the positive electrode material is greater than 80%, the peak temperature of thermal decomposition at a charging cut-off voltage of 4.3V is not less than 225°C, indicating that the positive electrode material has a higher peak temperature of thermal decomposition even under high pressure.

[0056] In some embodiments of the present application, the positive electrode material includes a core layer and a shell layer, the shell layer is coated on at least part of the surface of the core layer, and the thickness of the shell layer ranges from 10nm to 20nm; the composition of the positive electrode material is shown in formula (I):

[0057] Li m [Ni x Co y Mn z M a N b ]O 2 (I);

[0058] In the positive electrode material, the value ranges of m, x, y, z, a, and b are as follows: 0.98<m<1.05, 0.5<x<1, 0<y<0.2, 0<z<0.2, 0<a<0.1, x+y+z+a+b=1; wherein, element M is doped in the core layer, and element M includes at least one of Al, Ga, Mg, La, Y, Zn, V, and Sr; element N is doped in the shell layer, and element N includes at least one of Ti, Zr, Nb, Mo, Ta, W, and Ce.

[0059] The present invention provides a cathode material with nickel, cobalt and manganese as ternary elements, wherein the structure includes a core layer and a shell layer, and the core-shell structure can not only improve the stability of the overall structure of the cathode material and the diffusion rate of lithium ions, but also improve the stability of the surface structure of the cathode material; the cathode material is doped with element M and element N, wherein the diffusion rate of element M in the cathode material is greater than the diffusion rate of element N in the cathode material, and according to the diffusion rate of the doped element, it is ensured that element M is doped in the core layer and element N is doped in the shell layer.

[0060] The shell layer of the positive electrode material is wrapped around at least part of the surface of the core layer of the positive electrode material, and the shell layer is doped with element N. The doping of element N can effectively improve the stability of the surface structure of the positive electrode material, wherein the thickness range of the shell layer is controlled between 10nm-20nm, and the setting of this thickness is more conducive to the diffusion of lithium ions. Further preferably, the thickness range of the shell layer is 12nm-17nm.

[0061] The diffusion rate of element M in the positive electrode material is greater than the diffusion rate of element N in the positive electrode material. Element M diffuses relatively quickly in the positive electrode material, and is mainly evenly distributed in the core layer of the positive electrode material; element N diffuses relatively slowly in the positive electrode material, and is mainly doped in the shallow layer of the positive electrode material to form a shell structure, which is mainly used to improve the shallow layer stability of the material. The positive electrode material with a core-shell structure obtained by doping elements M and N has the characteristics of high strength, ability to withstand high voltage, and good safety performance. Among them, by doping element M in the core layer, the stability of the overall structure of the positive electrode material and the diffusion rate of lithium ions can be improved, and by doping element N in the shell layer, the stability of the surface structure of the positive electrode material can be improved.

[0062] In some embodiments of the present application, when the nickel content of the positive electrode material is 50%-80%, the tap density TD of the positive electrode material is ≥2.5 g / cm 3 ; and / or when the nickel content of the positive electrode material is 80%-90%, the tap density TD of the positive electrode material is ≥2.3g / cm 3 ; and / or when the nickel content of the positive electrode material is 90%-100%, the tap density of the positive electrode material TD ≥ 2.1g / cm 3 .

[0063] The value range of the nickel content in the positive electrode material is 0.5<x<1. When the nickel content of the positive electrode material is 50%-80%, the tap density TD of the positive electrode material is ≥2.5g / cm 3 ; When the nickel content of the positive electrode material is 80%-90%, the tap density of the positive electrode material TD ≥ 2.3g / cm 3 ; When the nickel content of the positive electrode material is 90%-100%, the tap density of the positive electrode material TD ≥ 2.1g / cm 3, indicating that the value range of the nickel content in this embodiment can ensure that the positive electrode material has a higher tap density. At this time, if the positive electrode material also has a higher strength, the prepared positive electrode sheet has a higher compaction density, thereby increasing the energy density of the battery. Among them, the higher the nickel content, the more difficult it is for the single crystal particles to grow during the sintering of the material, making the morphology of the positive electrode material difficult to control, which leads to a lower tap density; in addition, the higher the nickel content of the positive electrode material, the lower the lithium-nickel mixing ratio, which can improve the stability of the battery cycle, but at this time the tap density of the positive electrode material is also lower, and the energy density of the battery is also smaller. Therefore, it is necessary to select a suitable range of nickel content to ensure that the battery has good cycle performance and a higher energy density. Preferably, the nickel content of the positive electrode material is controlled between 70% and 90%.

[0064] In some embodiments of the present application, the lithium-nickel mixing ratio Li / Ni mixing of the positive electrode material has a numerical range of 0%<Li / Ni mixing<2%.

[0065] In the process of preparing positive electrode materials with single crystal morphology, a higher sintering temperature is required, but high temperature easily causes lithium-nickel mixing. A higher lithium-nickel mixing ratio not only easily leads to the aggravation of interface side reactions, but also reduces the capacity of the battery. Therefore, the numerical range of the lithium-nickel mixing ratio Li / Ni mixing of the positive electrode material is controlled between 0%<Li / Ni mixing<2%. A lower lithium-nickel mixing ratio can effectively improve the stability of the crystal structure, thereby improving the cycle stability of the positive electrode material. Further preferably, the numerical range of the lithium-nickel mixing ratio Li / Ni mixing of the positive electrode material is 0%<Li / Ni mixing<1.5%.

[0066] The embodiment of the present invention also provides a method for preparing a single crystal positive electrode material, the method for preparing the positive electrode material as described above, the method comprising the following steps: primary sintering: sintering a Li source, a Ni / Co / Mn ternary precursor, and an oxide containing element M to obtain a sintered product; secondary sintering: sintering the sintered product and a compound containing element N to obtain a positive electrode material; wherein the temperature curve of the primary sintering sequentially comprises a first temperature section T 1 , the second temperature section T 2 , the third temperature section T 3 And the fourth temperature section T 4 ; T 1 、T 2 、T 3 、T 4 The value ranges of T are as follows: 1 400℃-600℃; T 1 <T 2 ≤800℃; T 2+100℃<T 3 ≤1000℃;T 1 <T 4 ≤800℃; first temperature section T 1 , the second temperature section T 2 , the fourth temperature section T 4 The oxygen flux is greater than the third temperature section T 3 oxygen flux; element M includes at least one of Al, Ga, Mg, La, Y, Zn, V, and Sr; element N includes at least one of Ti, Zr, Nb, Mo, Ta, W, and Ce.

[0067] The preparation method for preparing positive electrode materials provided by the present invention is prepared by performing primary sintering and secondary sintering to obtain the required positive electrode materials. Among them, the Li source, the Ni / Co / Mn ternary precursor, and the oxide containing the M element are sintered once, and then the sintered product and the compound of the N element are sintered twice to finally prepare the positive electrode material. The diffusion rate of the element M in the ternary material is greater than that of the element N. According to the diffusion rate of the doped element in the ternary positive electrode material, step-by-step doping is performed, wherein the primary sintering is doped with the element with a high diffusion rate in the positive electrode material under high temperature conditions, and the secondary sintering is doped with the element with a slow diffusion rate in the positive electrode material under low temperature conditions to form a core-shell structure with good safety performance.

[0068] Through the two-step sintering process and combined with the doping of related elements to form a core-shell structure, the obtained single crystal positive electrode material has high safety performance, among which, the doping element M of the first sintering diffuses relatively quickly in the positive electrode material, and combined with the corresponding multi-stage sintering process, it is mainly evenly distributed in the core layer of the positive electrode material; the doping element N of the second sintering diffuses relatively slowly in the positive electrode material, and the sintering temperature is low, and it is mainly doped in the shallow layer of the positive electrode material to form a shell structure, which is mainly used to improve the shallow layer stability of the material. The positive electrode material with a core-shell structure obtained by combining a multi-step sintering process with doping elements has the characteristics of high strength, ability to withstand high voltage, and good safety performance.

[0069] Specifically, through multi-step doping, elements that diffuse faster in the ternary material are first doped at a higher temperature, and then elements that diffuse slower in the ternary material are doped at a lower temperature. The faster diffusing elements are distributed in the core of the matrix, improving the structural stability of the material and the diffusion rate of lithium ions, and the slower diffusing elements are distributed in the shallow surface layer of the matrix, improving the stability of the surface structure.

[0070] Preferably, the primary sintering specifically includes: sintering the Li source, Ni / Co / Mn ternary precursor, and oxide containing M element under oxygen atmosphere, and then rolling, crushing, screening and grading to obtain a sintered product; the secondary sintering specifically includes: mixing the sintered product and the compound containing N element evenly, and sintering under oxygen atmosphere to obtain a positive electrode material. Compared with the preparation of polycrystalline materials, the sintering temperature for preparing single crystal materials is generally relatively higher; during the sintering process of single crystal materials, the primary particles will grow and the secondary particles will also stick together, so rolling, crushing, screening and grading operations are required after sintering.

[0071] A positive electrode material with a large single crystal size can be prepared under high temperature conditions. By setting different temperature sections, the lithium-nickel mixing and grain boundary phenomena caused by high temperature can be reduced. The overall lithium-nickel mixing degree of the positive electrode material is low, the dispersion degree is high, and it has a high compaction density and electrochemical performance. The element M with a faster diffusion rate is doped in the primary sintering process to make it evenly distributed in the material body. By setting four sintering temperature sections in the primary sintering step and limiting the sintering temperature, a single crystal positive electrode material with high strength is formed.

[0072] Among them, the second temperature section T 2 The role of is to form a layered and rock salt composite phase, which is more conducive to the formation of single crystals, reduce the generation of grain boundaries, and increase the dispersion of single crystals; the third temperature section T 3 The role of is to reduce the time and ventilation volume of the high temperature section, and to reduce the degree of lithium-nickel mixing. Among them, the temperature value of this temperature section is the highest, and its purpose is to promote more uniform growth of single crystals, and reducing the ventilation volume is to reduce oxidation during the growth process; the fourth temperature section T 4 The function is to relieve the stress in the high temperature section and rearrange it, thereby increasing the strength of the positive electrode material.

[0073] By limiting the size of the oxygen flux during the sintering process, it is beneficial to form a single crystal positive electrode material with high strength, wherein in the third temperature section T of the primary sintering 3 The oxygen flux needs to be reduced to ensure the first temperature section T 1 , the second temperature section T 2 , the fourth temperature section T 4 The oxygen flux is greater than the third temperature section T 3 The oxygen flux is reduced, thereby helping to reduce the oxidation of the single crystal during the growth process. Preferably, the first temperature section T 1 The oxygen flux is 10L / min-40L / min; the second temperature section T 2 The oxygen flux is 10L / min-40L / min; the third temperature section T 3The oxygen flux is 0L / min-20L / min; the fourth temperature section T 4 The oxygen flux is 10L / min-40L / min; the oxygen flux in the heating section of the primary sintering is 10L / min-40L / min; the oxygen flux in the cooling section of the primary sintering is 10L / min-40L / min.

[0074] In some embodiments of the present application, the first temperature section T 1 The maintenance time is 2h-8h; and / or the second temperature section T 2 The maintenance time is 2h-8h; and / or the third temperature section T 3 The maintenance time is 2h-6h; and / or the fourth temperature section T 4 The holding time is 2h-8h; and / or the heating rate of the first sintering is 1℃ / min-5℃ / min; and / or the heating rate of the second sintering is 1℃ / min-5℃ / min; and / or the sintering temperature of the second sintering is 700℃-900℃; and / or the sintering time of the second sintering is 8h-12h.

[0075] The process parameters of the maintenance time of the four sintering temperature sections in one sintering are related to the compaction density and strength of the positive electrode material. The selection of the maintenance time is to make the growth of the single crystal positive electrode material more uniform, better dispersibility, higher strength, more uniform internal stress distribution, and better electrochemical performance. Therefore, this embodiment provides a preferred maintenance time range to obtain the positive electrode material claimed in this application. Further preferably, the first temperature section T 1 The maintenance time is 3h-6h; the second temperature section T 2 The maintenance time is 3h-6h; the third temperature section T 3 The maintenance time is 3h-5h; the fourth temperature section T 4 The maintenance time is 3h-6h.

[0076] According to the diffusion rate of the doping elements in the positive electrode material, doping is carried out in steps, wherein the elements with high diffusion rate in the positive electrode material are doped under high temperature conditions in the first sintering, and the elements with slow diffusion rate in the positive electrode material are doped under low temperature conditions in the second sintering, forming a core-shell structure with good safety performance. The doping element M in the first sintering diffuses relatively quickly in the positive electrode material, and combined with the corresponding multi-stage sintering process, it is mainly evenly distributed in the core layer of the positive electrode material; the doping element N in the second sintering diffuses relatively slowly in the positive electrode material, and the sintering temperature is relatively low, and it is mainly doped in the shallow layer of the positive electrode material to form a shell structure, which is mainly used to improve the shallow surface stability of the material. The positive electrode material obtained by two-step sintering has the characteristics of high strength, ability to withstand high voltage, and good safety performance.

[0077] During the preparation of positive electrode materials, a too fast sintering heating rate will lead to uneven material growth and internal stress distribution, while a too slow heating rate will lead to a longer sintering cycle and increased energy consumption. Therefore, in this embodiment, the heating rate of the primary sintering is controlled at 1°C / min-5°C / min, and the heating rate of the secondary sintering is controlled at 1°C / min-5°C / min. Further preferably, the heating rate of the primary sintering is 2°C / min-4°C / min; the heating rate of the secondary sintering is 2°C / min-4°C / min; the sintering temperature of the secondary sintering is 750°C-850°C; and the sintering time of the secondary sintering is 9h-11h.

[0078] The embodiment of the present invention further provides a lithium ion battery, the lithium ion battery includes the positive electrode material as described above, and the lithium ion battery has the same beneficial effects as the positive electrode material as described above, so it is not repeated here. The compaction density of the positive electrode sheet prepared by the positive electrode material is 3.5g / cm 3 -4.0g / cm 3 .

[0079] Example 1

[0080] This embodiment provides a method for preparing a positive electrode material, comprising the following steps:

[0081] S1: The element M is Sr and Al, the molar ratio of Li:(Ni+Co+Mn)=1.05:1, the amount of Sr added is 500ppm, the amount of Al added is 1000ppm, and lithium hydroxide, Ni 0.83 Co 0.06 Mn 0.11 (OH) 2 , SrO and Al 2 O 3 . Mix the above raw materials evenly in a high-speed mixer, put the mixed raw materials into a sagger and sinter once in a high-temperature atmosphere box furnace. In an oxygen atmosphere, heat up to 500°C at a heating rate of 2°C / min and keep warm for 4 hours; heat up to 780°C and keep warm for 6 hours; heat up to 950°C and keep warm for 2 hours; cool down to 780°C and keep warm for 6 hours. Except for the third temperature section, the ventilation volume is 10L / min, and the ventilation volumes of the other three temperature sections are all 20L / min. The sintered material is then crushed by jaw crusher, roller, crushing, screening and grading to obtain the sintered product Li 1.03 Ni 0.83 Co 0.056 Mn 0.11 Al 0.0035 Sr 0.0005 O 2 ;

[0082] S2: Element N is Zr, and the amount of Zr added is 3000ppm. Weigh the above sintered product and nano ZrO 2 After mixing evenly, the mixed raw materials were put into a sagger and sintered twice in a high-temperature atmosphere box furnace. In an oxygen atmosphere, the temperature was raised to 800°C at a heating rate of 2°C / min and kept at this temperature for 8 hours to obtain a single crystal positive electrode material Li with good uniformity and dispersion and high tap / compact density. 1.03 Ni 0.83 Co 0.053 Mn 0.11 Al 0.0035 Sr 0.0005 Zr 0.003 O 2 .

[0083] The morphology of the positive electrode material provided in this embodiment 1 is shown in Figure 1 , see the cross-sectional view Figure 2 .

[0084] Example 2

[0085] This embodiment provides a method for preparing a positive electrode material. The specific steps are as described in Embodiment 1, except that in step S1, the element M is Sr, Al, and La, the amount of Sr added is 500 ppm, the amount of Al added is 1000 ppm, and the amount of La added is 1000 ppm.

[0086] Example 3

[0087] This embodiment provides a method for preparing a positive electrode material. The specific steps are as shown in Embodiment 1, except that in step S2, the element N is Ce, and the amount of Ce added is 3000 ppm.

[0088] Example 4

[0089] This embodiment provides a method for preparing a positive electrode material. The specific steps are as shown in Example 1, except that the Ni / Co / Mn ternary precursor in step S1 is Ni 0.9 Co 0.05 Mn 0.05 (OH) 2 , the maximum sintering temperature is 940℃.

[0090] Example 5

[0091] This embodiment provides a method for preparing a positive electrode material. The specific steps are as shown in Example 1, except that the Ni / Co / Mn ternary precursor in step S1 is Ni 0.6 Co 0.1 Mn 0.3 (OH) 2 , the maximum sintering temperature is 970℃.

[0092] Comparative Example 1

[0093] This comparative example provides a method for preparing a positive electrode material. The specific steps refer to Example 1, except that the sintering process in step S1 is to heat up to 500°C at a heating rate of 2°C / min, keep the temperature for 3 hours, then heat up to 950°C, keep the temperature for 12 hours, and then cool naturally.

[0094] The morphology of the positive electrode material provided in this comparative example 1 is shown in Figure 3 , see the interface diagram Figure 4 .

[0095] Comparative Example 2

[0096] This comparative example provides a method for preparing a positive electrode material, comprising the following steps:

[0097] The molar ratio of Li:(Ni+Co+Mn)=1.05:1, the amount of Sr added is 500ppm, the amount of Al added is 1000ppm, and the amount of Zr added is 3000ppm. Lithium hydroxide, Ni 0.83 Co 0.06 Mn 0.11 (OH) 2 、SrO、Al 2 O 3 and ZrO 2 The above raw materials were mixed evenly in a high-speed mixer, and the mixed raw materials were put into a sagger and sintered in a high-temperature atmosphere box furnace. In an oxygen atmosphere, the temperature was increased to 500°C at a heating rate of 2°C / min, and kept warm for 4 hours; the temperature was increased to 780°C and kept warm for 6 hours; the temperature was increased to 950°C and kept warm for 2 hours; the temperature was lowered to 780°C and kept warm for 6 hours. Except for the ventilation volume of the third temperature section of 10L / min, the ventilation volume of the other three temperature sections was 20L / min. Then the sintered material was crushed by jaw crusher, roller, crushing and screening to obtain the positive electrode material.

[0098] The electrochemical performance of the positive electrode materials obtained according to Examples 1-5 and Comparative Examples 1-2 was tested, and the testing method was as follows:

[0099] Button capacity: At 25°C and normal pressure (0.1MPa), the single crystal ternary positive electrode material, conductive carbon black, and binder polyvinylidene fluoride (PVDF) of each embodiment and comparative example were weighed in a mass percentage ratio of 95:3:2, and fully stirred and mixed in N-methylpyrrolidone solvent to obtain positive electrode slurry, and the positive electrode slurry was coated on aluminum foil, and after drying and cold pressing, a positive electrode sheet including a positive electrode active layer with a thickness of 100μm was obtained; the positive electrode sheet, lithium sheet, isolation membrane and electrolyte were assembled into a button battery in a button box. Under the condition of 0.2C constant current charging, when the nickel content of the positive electrode material is 0.5-0.7, the charging cut-off voltage is 4.45V; when the nickel content of the positive electrode material is 0.8-1, the charging cut-off voltage is 4.3V, and then constant voltage charging is performed under the cut-off voltage condition until the current is less than 0.05C. The charging capacity at this time is recorded as the first cycle charging capacity. After standing for 5 minutes, it is discharged at a constant current of 0.2C to a voltage of 2.8V. The discharge capacity this time is recorded as the battery first cycle discharge specific capacity, which is also the initial capacity.

[0100] Full electric cycle: According to the method of the charge capacity test, the positive electrode material is coated into a positive electrode sheet, and the negative electrode is made of graphite, and is combined with a diaphragm polyethylene and an electrolyte (the electrolyte is LiPF 6 The full battery was composed of a 1C charge and discharge rate (EC / DMC as the solvent) and cycled. The capacity of each cycle was compared with the initial capacity to confirm the capacity retention rate. At 45°C, the capacity retention rate was calculated after 300 cycles.

[0101] Cell expansion: Assemble the whole battery according to the method in the full electric cycle test, fully charge the battery to the set voltage, use the PPG battery thickness gauge to test the battery thickness, then place the battery in a 70℃ constant temperature box for 28 days, take out the battery, use the PPG battery thickness gauge to test the battery thickness at this time, and use the following formula to calculate the battery thickness expansion rate, battery thickness expansion rate = (battery thickness after constant temperature - battery thickness before constant temperature) / battery before constant temperature. The size of the battery thickness expansion rate can reflect the gas production performance of the battery. The smaller the battery thickness expansion rate, the less gas production.

[0102] Particle size test: The powder is first subjected to external supersizing, and then the particle size test is performed using a Malvern 2000 or 3000 laser particle size analyzer to obtain the particle size data.

[0103] Tap density: Fix the graduated cylinder containing positive electrode material on the mechanical vibration device. The vibration motor drives the mechanical vibration device to vibrate vertically up and down. The graduated cylinder containing powder or particles vibrates rhythmically with the mechanical vibration device. As the number of vibrations increases, the powder or particles in the graduated cylinder are gradually vibrated. After the number of vibrations reaches the set number, the mechanical vibration device stops vibrating and the volume of the graduated cylinder is read. According to the definition of density, that is, mass divided by volume, the density after tapping is calculated, which is the tap density.

[0104] Positive electrode material component test: The actual chemical composition of the positive electrode material was determined by ICP-AES. The results showed that the actual chemical composition of each finished product was basically consistent with the designed proportions of each sample in Table 1.

[0105] Element distribution test: The positive electrode material is first ion cut and then transferred to the morphology testing equipment Hitachi Regulus 8100 / SU 8010 for cross-sectional morphology and element distribution testing.

[0106] Pole sheet compaction: Pole sheet compaction density = pole sheet surface density / (pole sheet thickness after rolling - current collector thickness).

[0107] Table 1 Physical and chemical parameters and process parameters of the embodiments and comparative examples

[0108]

[0109] Table 2 Electrochemical performance of examples and comparative examples

[0110]

[0111] It can be seen from Table 1 and Table 2 that the positive electrode material prepared in the embodiment has better capacity, high temperature cycle and gas production performance.

[0112] like Figure 1-4 As shown, Figure 1 is an electron microscope image of the positive electrode material in Example 1, Figure 2 is the EDS image of the cross section of the positive electrode material in Example 1, Figure 3 This is the electron microscope image of the positive electrode material in Comparative Example 1. Figure 4 This is an EDS image of the cross section of the positive electrode material in Comparative Example 1. The positive electrode material prepared according to the preparation method of Example 1 has a higher degree of dispersion, better uniformity of the material, and the element distribution in the material has an obvious core-shell structure; the positive electrode material prepared by the conventional preparation method in Comparative Example 1 has obvious agglomeration and irregular morphology.

[0113] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a single crystal positive electrode material, It is characterized in that When the positive electrode material is subjected to a pressure of 8T-10T, the particle size volume distribution of the positive electrode material is a unimodal distribution; The positive electrode material comprises a core layer and a shell layer, wherein the shell layer covers at least a portion of the surface of the core layer; the composition of the positive electrode material is as shown in formula (I): Li m [Ni x Co y Mr z M a N b ]O 2 (Ⅰ); In the positive electrode material, the value ranges of m, x, y, z, a, and b are as follows: 0.98<m<1.05, 0.5<x<1, 0<y<0.2, 0<z<0.2, 0<a<0.1, x+y+z+a+b=1; Wherein, the element M is doped into the core layer, and the element M includes at least one of Al, Ga, Mg, La, Y, Zn, V, and Sr; Element N is doped into the shell layer, and the element N includes at least one of Ti, Zr, Nb, Mo, Ta, W, and Ce; The compaction density PD of the positive electrode material powder is in the range of PD ≥ 3.72 g / cm 3 ; The method for preparing the single crystal positive electrode material comprises the following steps: Primary sintering: sintering the Li source, Ni / Co / Mn ternary precursor, and the oxide containing the element M to obtain a sintered product; Secondary sintering: secondary sintering the sintered product and the compound containing element N to obtain the positive electrode material; The temperature curve of the primary sintering includes the first temperature section T 1 , the second temperature section T 2 , the third temperature section T 3 and the fourth temperature section T 4 ; T 1 , T 2 , T 3 , T 4 The value ranges are as follows: T 1 is 400 °C - 600 °C; T 1 <T 2 ≤ 800 °C; T 2 +100 °C < T 3 ≤ 1000 °C; T 1 <T 4 ≤ 800 °C; The first temperature section T 1 The second temperature section T 2 The fourth temperature section T 4 The oxygen flux is greater than the third temperature section T 3 of oxygen flux.

2. The preparation method according to claim 1, It is characterized in that Under the condition that the positive electrode material is subjected to a pressure of 8T-10T, the particle size D50 of the positive electrode material before being subjected to the pressure is 1 Particle size after pressure D50 2 The numerical range of the change difference △D50 is 0μm<△D50<0.1μm; Wherein, the particle size D50 of the positive electrode material before being subjected to pressure 1 The range is 4μm<D50 1 <7μm.

3. The preparation method according to claim 1, It is characterized in that The compaction density CD of the electrode sheet prepared by the positive electrode material is in the range of CD ≥ 3.55 g / cm 3 .

4. The preparation method according to claim 1, It is characterized in that When the nickel content of the positive electrode material is 50%-80%, the peak temperature of thermal decomposition at a charge cut-off voltage of 4.45V is not less than 250°C; and / or When the nickel content of the positive electrode material is greater than 80%, the thermal decomposition peak temperature at a charge cut-off voltage of 4.3 V is not less than 225° C.

5. The preparation method according to claim 1, It is characterized in that The thickness of the shell layer is in the range of 10 nm to 20 nm.

6. The preparation method according to claim 1, It is characterized in that When the nickel content of the positive electrode material is 50%-80%, the tap density TD of the positive electrode material is ≥2.5g / cm 3 ; and / or When the nickel content of the positive electrode material is 80%-90%, the tap density TD of the positive electrode material is ≥2.3 g / cm 3 ; and / or When the nickel content of the positive electrode material is 90%-100%, the tap density TD of the positive electrode material is ≥2.1 g / cm 3 .

7. The preparation method according to claim 1, It is characterized in that The lithium-nickel mixing ratio Li / Ni mixing of the positive electrode material has a numerical range of 0%<Li / Ni mixing<2%.

8. The preparation method according to claim 1, It is characterized in that The first temperature section T 1 The maintenance time is 2h-8h; and / or The second temperature section T 2 The maintenance time is 2h-8h; and / or The third temperature section T 3 The maintenance time is 2h-6h; and / or The fourth temperature section T 4 The maintenance time is 2h-8h; and / or The heating rate of the primary sintering is 1°C / min-5°C / min; and / or The heating rate of the secondary sintering is 1°C / min-5°C / min; and / or The sintering temperature of the secondary sintering is 700° C.-900° C.; and / or The sintering time of the secondary sintering is 8h-12h.

9. A single crystal positive electrode material, It is characterized in that The positive electrode material is prepared by the preparation method according to any one of claims 1 to 8.

10. A lithium ion battery, It is characterized in that Comprising the positive electrode material as claimed in claim 9.