Large-particle positive electrode material precursor, preparation method, positive electrode material and application

By controlling the addition rate of metal mixed salt solution, precipitant solution and complexing agent solution in stages, the problem of uneven particle size distribution of the precursor of large-particle positive electrode material is solved, and the excellent electrochemical performance of the battery is achieved.

CN118908306APending Publication Date: 2024-11-08GEM CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410990008.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The particle size distribution of the existing large-particle positive electrode material precursors is uneven, resulting in poor electrochemical performance of the battery.

Method used

Using a mixing process divided into at least three stages, the addition speed of metal mixed salt solution, precipitant solution and complexing agent solution increases or decreases in succession to control the particle size distribution of the precursor of the large-particle positive electrode material to achieve single-peak distribution .

Benefits of technology

The obtained large-particle positive electrode material precursor has uniform particle size distribution and excellent electrochemical performance, which improves the first-effect, cycle stability and rate performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908306A_ABST
    Figure CN118908306A_ABST
Patent Text Reader

Abstract

The invention provides a large-particle positive electrode material precursor and a preparation method thereof, and a positive electrode material and application thereof, the preparation method comprises the following steps: in a protective atmosphere, mixing a metal mixed salt solution, a precipitator solution and a complexing agent solution into a reaction base solution to obtain the large-particle positive electrode material precursor; the mixing is carried out in at least three stages, and the adding speeds of the metal mixed salt solution, the precipitator solution and the complexing agent solution are synchronously and sequentially increased or sequentially decreased after entering the next stage from the previous stage. According to the invention, the size control of the large-particle positive electrode material precursor is realized, and the large-particle positive electrode material precursor with uniform particle size distribution and unimodal particle size distribution diagram is obtained; therefore, the battery prepared from the obtained large-particle positive electrode material precursor shows excellent electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of batteries, and relates to a method for preparing a large-particle positive electrode material precursor, and in particular to a large-particle positive electrode material precursor and a preparation method, a positive electrode material and an application thereof. Background Art

[0002] Precursors are key materials for preparing battery positive electrodes. The particle size distribution, morphology and crystal structure of the precursors restrict the electrochemical performance of battery positive electrode materials. However, in the overflow method, since the total number of particles decreases over time, the total surface area decreases as the particles continue to grow, and the sites available for the growth of newly generated hydroxides decrease. If a stable feed flow rate is maintained, the actual growth rate limit of the particles in the reactor will eventually be exceeded, resulting in large-scale nucleation to generate new surface area and growth sites to accommodate the excess supply of reactants. In the dense method, if a stable feed flow rate is maintained, it is difficult for the particles to continue to grow.

[0003] CN116986636A discloses a sodium ion battery and its iron-based multi-element positive electrode material and precursor and preparation method, belonging to the field of battery technology. The preparation of the iron-based multi-element positive electrode material precursor includes: reacting a base liquid, a precipitant solution, a complexing agent solution and a metal salt aqueous solution, and stopping the addition of materials when the material growth particle size reaches a preset value; the ammonia concentration in the base liquid is 1.5g / L-16g / L, and the pH value is 9.5-12; the precipitant solution controls the pH value range of the system during the seed synthesis process to be 9.5-12, and the complexing agent solution controls the ammonia concentration of the system to be 0g / L-16g / L; the reaction temperature is 30℃-70℃.

[0004] CN113479942A discloses a ternary positive electrode material precursor with a core-shell structure, a preparation method thereof, an automatic control feeding system and application. The preparation method comprises: mixing a complexing agent, an alkaline precipitant and three metal salts, reacting, and sequentially undergoing a core-making reaction stage and a shell-making reaction stage; by establishing a response relationship between the flow rate of the alkaline precipitant and the pH of the reaction system in the coprecipitation reaction, the relative stability of the pH in the reaction system is achieved. At the same time, by setting two different pH values ​​in the core-making reaction stage and the shell-making reaction stage, the preparation of the core-shell precursor is achieved, and the purpose of controlling the microstructure of the core-shell material is achieved.

[0005] The preparation methods of large-particle positive electrode material precursors disclosed in the prior art all have certain defects, such as uneven particle size distribution of the prepared large-particle positive electrode material precursors and multi-peak distribution of particle size distribution. Therefore, it is very important to develop and design a new type of large-particle positive electrode material precursor and preparation method, positive electrode material and application. Summary of the invention

[0006] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a large-particle positive electrode material precursor and a preparation method, a positive electrode material and an application. In the present invention, the mixing process is divided into at least three stages, and after the previous stage to the next stage, the addition speed of the metal mixed salt solution, the precipitant solution and the complexing agent solution is synchronously increased or decreased in sequence, thereby achieving size control of the large-particle positive electrode material precursor, and obtaining a large-particle positive electrode material precursor with uniform particle size distribution and a particle size distribution diagram showing a single peak distribution; therefore, the battery prepared with the obtained large-particle positive electrode material precursor exhibits excellent electrochemical performance.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a method for preparing a large-particle positive electrode material precursor, the preparation method comprising:

[0009] In a protective atmosphere, a metal mixed salt solution, a precipitant solution and a complexing agent solution are mixed into a reaction base liquid to obtain a large-particle positive electrode material precursor;

[0010] The mixing is carried out in at least three stages. Each time after entering the next stage from the previous stage, the adding speed of the metal mixed salt solution, the precipitant solution and the complexing agent solution is synchronously increased or decreased in sequence.

[0011] In the present invention, the mixing process is divided into at least three stages, and after the previous stage to the next stage, the addition speed of the metal mixed salt solution, the precipitant solution and the complexing agent solution is synchronously increased or decreased in sequence, thereby achieving size control of the large-particle positive electrode material precursor, and obtaining a large-particle positive electrode material precursor with uniform particle size distribution and a particle size distribution diagram showing a single peak distribution; therefore, the battery prepared with the obtained large-particle positive electrode material precursor exhibits excellent electrochemical performance.

[0012] Preferably, the mixing is carried out in a first stage, a second stage and a third stage, and the adding speeds of the mixed salt solution, the precipitant solution and the complexing agent solution in the first stage, the second stage and the third stage are synchronously decreased or increased successively.

[0013] Preferably, the adding speeds of the mixed salt solution, the precipitant solution and the complexing agent solution in the first stage, the second stage and the third stage are synchronously decreased in sequence.

[0014] Preferably, in the first stage, the hourly feed rate of the mixed salt solution is 2-4% of the available capacity of the reaction container, the hourly feed rate of the precipitant solution is 0.5-2% of the available capacity of the reaction container, and the hourly feed rate of the complexing agent solution is 0.1%-0.5% of the available capacity of the reaction container.

[0015] The hourly feed rate of the mixed salt solution in the first stage of the present invention is 2-4% of the available capacity of the reaction container, for example, it can be 2%, 2.2%, 2.4%, 2.6%, 2.8%, 3%, 3.2%, 3.4%, 3.6%, 3.8% or 4%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] In the present invention, the feed rate of the precipitant solution per hour in the first stage is 0.5-2% of the available capacity of the reaction container, for example, it can be 0.5%, 0.7%, 0.9%, 1%, 1.2%, 1.4%, 1.6%, 1.8% or 2%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] In the present invention, the feeding amount of the complexing agent solution per hour in the first stage is 0.1-0.5% of the available capacity of the reaction container, for example, it can be 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45% or 0.5%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] Preferably, the first stage ends when the particle size distribution diagram of the precipitate changes suddenly from multi-peaks to single peak.

[0019] Preferably, the addition rates of the mixed salt solution, the precipitant solution and the complexing agent solution in the second stage are independently 0.5 to 0.9 times that of the first stage, for example, 0.5 times, 0.55 times, 0.6 times, 0.65 times, 0.7 times, 0.75 times, 0.8 times, 0.85 times or 0.9 times, but are not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, the D50 particle size of the precipitate is tested every hour in the second stage, and the test ends when the D50 particle size of the precipitate increases by no less than 0.2 μm compared with the D50 particle size of the last sampling test.

[0021] In the second stage of the present invention, the D50 particle size of the precipitate is detected once every hour to obtain the D50 particle size of each detection. When the D50 particle size obtained by the last detection is larger than the D50 particle size obtained by the sampling test in the previous hour by not less than 0.2 μm, the second stage is stopped; wherein the D50 particle size obtained by the last detection is larger than the D50 particle size obtained by the sampling test in the previous hour by not less than 0.2 μm, for example, it can be 0.2 μm, 0.22 μm, 0.24 μm, 0.26 μm, 0.28 μm, 0.3 μm, 0.32 μm, 0.35 μm, 0.4 μm, 0.45 μm or 0.5 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0022] Preferably, the addition rates of the mixed salt solution, the precipitant solution and the complexing agent solution in the third stage are independently 0.1 to 0.9 times that of the second stage, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8 or 0.9 times, but are not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] Preferably, the adding speeds of the mixed salt solution, the precipitant solution and the complexing agent solution in the first stage, the second stage and the third stage are increased synchronously and successively.

[0024] Preferably, in the first stage, the hourly feed rate of the mixed salt solution is 2-4% of the available capacity of the reaction container, the hourly feed rate of the precipitant solution is 0.5-2% of the available capacity of the reaction container, and the hourly feed rate of the complexing agent solution is 0.1%-0.5% of the available capacity of the reaction container.

[0025] The hourly feed rate of the mixed salt solution in the first stage of the present invention is 2-4% of the available capacity of the reaction container, for example, it can be 2%, 2.2%, 2.4%, 2.6%, 2.8%, 3%, 3.2%, 3.4%, 3.6%, 3.8% or 4%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] In the present invention, the feed rate of the precipitant solution per hour in the first stage is 0.5-2% of the available capacity of the reaction container, for example, it can be 0.5%, 0.7%, 0.9%, 1%, 1.2%, 1.4%, 1.6%, 1.8% or 2%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] In the present invention, the feeding amount of the complexing agent solution per hour in the first stage is 0.1-0.5% of the available capacity of the reaction container, for example, it can be 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45% or 0.5%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] Preferably, the first stage ends when the particle size distribution diagram of the precipitate changes suddenly from multi-peaks to single peak.

[0029] Preferably, the addition rate of the mixed salt solution, the precipitant solution and the complexing agent solution in the second stage is independently 1.1 to 3.5 times that of the first stage, for example, it can be 1.1 times, 1.3 times, 1.5 times, 1.7 times, 1.9 times, 2 times, 2.2 times, 2.4 times, 2.6 times, 2.8 times, 3 times, 3.2 times, 3.4 times or 3.5 times, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] Preferably, the D50 particle size of the precipitate is tested every hour in the second stage, and the test ends when the D50 particle size of the precipitate increases by no less than 0.2 μm compared with the D50 particle size of the last sampling test.

[0031] In the second stage of the present invention, the D50 particle size of the precipitate is detected once every hour to obtain the D50 particle size of each detection. When the D50 particle size obtained by the last detection is larger than the D50 particle size obtained by the sampling test in the previous hour by not less than 0.2 μm, the second stage is stopped; wherein the D50 particle size obtained by the last detection is larger than the D50 particle size obtained by the sampling test in the previous hour by not less than 0.2 μm, for example, it can be 0.2 μm, 0.22 μm, 0.24 μm, 0.26 μm, 0.28 μm, 0.3 μm, 0.32 μm, 0.35 μm, 0.4 μm, 0.45 μm or 0.5 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0032] Preferably, the addition rate of the mixed salt solution, the precipitant solution and the complexing agent solution in the third stage is independently 1.1 to 5.5 times that of the second stage, for example, it can be 1.1 times, 1.3 times, 1.5 times, 1.7 times, 1.9 times, 2 times, 2.2 times, 2.4 times, 2.6 times, 2.8 times, 3 times, 3.2 times, 3.4 times, 3.6 times, 3.8 times, 4.2 times, 4.6 times, 4.8 times, 5.2 times or 5.5 times, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] Preferably, the metal mixture solution in the first stage also includes an antioxidant with a concentration of 0.1 to 0.3 g / L, for example, it can be 0.1 g / L, 0.12 g / L, 0.14 g / L, 0.16 g / L, 0.18 g / L, 0.2 g / L, 0.24 g / L, 0.26 g / L, 0.28 g / L or 0.3 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the addition of the metal mixed salt solution, the precipitant solution and the complexing agent solution in the first stage is accompanied by stirring at a speed of 600 to 1000 rpm, for example, 600 rpm, 650 rpm, 700 rpm, 750 rpm, 800 rpm, 850 rpm, 900 rpm, 950 rpm or 1000 rpm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] Preferably, the metal mixture solution in the second stage also includes an antioxidant with a concentration of 0.1 to 0.5 g / L, for example, it can be 0.1 g / L, 0.15 g / L, 0.2 g / L, 0.25 g / L, 0.3 g / L, 0.35 g / L, 0.4 g / L, 0.45 g / L or 0.5 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] Preferably, the addition of the metal mixed salt solution, the precipitant solution and the complexing agent solution in the second stage is accompanied by stirring at a speed of 600 to 800 rpm, for example, 600 rpm, 620 rpm, 640 rpm, 660 rpm, 680 rpm, 700 rpm, 720 rpm, 740 rpm, 760 rpm, 780 rpm or 800 rpm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] Preferably, the metal mixture solution in the third stage also includes an antioxidant with a concentration of 0.1 to 1 g / L, for example, it can be 0.1 g / L, 0.2 g / L, 0.3 g / L, 0.4 g / L, 0.5 g / L, 0.6 g / L, 0.7 g / L, 0.8 g / L, 0.9 g / L or 1 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] In the present invention, by controlling the added antioxidant, the oxidation of the metal mixed salt solution is effectively inhibited, thereby improving the structural stability and tap density of the obtained large-particle positive electrode material precursor, so that the battery prepared with the large-particle positive electrode material precursor exhibits better electrochemical performance.

[0039] Preferably, the addition of the metal mixed salt solution, the precipitant solution and the complexing agent solution in the third stage is accompanied by stirring at a speed of 400 to 600 rpm, for example, 400 rpm, 420 rpm, 440 rpm, 460 rpm, 480 rpm, 500 rpm, 520 rpm, 540 rpm, 560 rpm, 580 rpm or 600 rpm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] Preferably, the reaction base liquid comprises a solvent, a precipitant and a complexing agent, and the temperature of the reaction base liquid is 40-60° C. and the pH is 10-12.

[0041] The temperature of the reaction base liquid in the present invention is 40-60°C, for example, it can be 40°C, 42°C, 44°C, 46°C, 48°C, 50°C, 52°C, 54°C, 56°C, 58°C or 60°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] The pH of the reaction base solution in the present invention is 10-12, for example, it can be 10, 10.2, 10.4, 10.6, 10.8, 11, 11.2, 11.4, 11.6, 11.8 or 12, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] Preferably, during the entire mixing process, the pH of the mixed solution of the reaction base liquid, the metal mixed salt solution, the precipitant solution and the complexing agent solution is controlled to be 9.5-10.8, for example, it can be 9.5, 9.6, 9.7, 9.8, 9.9, 10, 10.1, 10.2, 10.3, 10.4, 10.5, 10.6, 10.7 or 10.8, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] Preferably, the total concentration of metal ions in the metal mixed salt solution is 2 to 3 mol / L, for example, 2 mol / L, 2.2 mol / L, 2.4 mol / L, 2.6 mol / L, 2.8 mol / L or 3 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] Preferably, the concentration of the precipitant in the precipitant solution is 30-35wt%, for example, it can be 30wt%, 31wt%, 32wt%, 33wt%, 34wt% or 35wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] Preferably, the concentration of the complexing agent in the complexing agent solution is 0.1-0.5 mol / L, for example, it can be 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L, 0.3 mol / L, 0.35 mol / L, 0.4 mol / L, 0.45 mol / L or 0.5 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0047] Preferably, the metal salt in the metal mixed salt solution includes a combination of at least two of nickel salts, iron salts, manganese salts or cobalt salts, for example, it can be a combination of nickel salts, iron salts and manganese salts, a combination of nickel salts, iron salts and cobalt salts, or a combination of nickel salts, iron salts, manganese salts and cobalt salts.

[0048] Preferably, the precipitant in the reaction base liquid and the precipitant solution independently includes any one of sodium hydroxide, potassium hydroxide or calcium hydroxide or a combination of at least two thereof. Typical but non-limiting combinations include a combination of sodium hydroxide and potassium hydroxide, a combination of potassium hydroxide and calcium hydroxide, and a combination of sodium hydroxide, potassium hydroxide and calcium hydroxide.

[0049] Preferably, the complexing agent in the reaction base solution and the complexing agent solution independently includes any one of ammonia, oxalic acid or EDTA or a combination of at least two of them. Typical but non-limiting combinations include a combination of ammonia and oxalic acid, a combination of oxalic acid and EDTA, or a combination of ammonia, oxalic acid and EDTA.

[0050] Preferably, the solvents in the reaction base solution, the metal mixed salt solution, the precipitant solution and the complexing agent solution each independently include water.

[0051] Preferably, the antioxidant includes but is not limited to ascorbic acid.

[0052] In a second aspect, the present invention provides a large-particle positive electrode material precursor, which is obtained by the preparation method described in the first aspect.

[0053] Preferably, the D50 particle size of the large-particle positive electrode material precursor is 10 to 15 μm, for example, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm or 15 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0054] Preferably, the specific surface area of ​​the large-particle positive electrode material precursor is 9 to 15 m 2 / g, for example, it can be 9m 2 / g, 10m 2 / g, 11m 2 / g, 12m2 / g, 13m 2 / g, 14m 2 / g or 15m 2 / g, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0055] Preferably, the tap density of the large-particle positive electrode material precursor is 1.5 to 2.5 g / cm 3 , for example, it can be 1.5 g / cm 3 , 1.6g / cm 3 , 1.7g / cm 3 , 1.8g / cm 3 , 1.9g / cm 3 , 2g / cm 3 , 2.1g / cm 3 , 1.5g / cm 3 、.

[0056] In a third aspect, the present invention provides a large-particle positive electrode material, which is prepared from the large-particle positive electrode material precursor described in the second aspect.

[0057] In a fourth aspect, the present invention provides a battery, comprising the large-particle positive electrode material described in the third aspect.

[0058] The batteries described in the present invention include lithium batteries and sodium batteries.

[0059] Compared with the prior art, the present invention has the following beneficial effects:

[0060] (1) In the present invention, the mixing process is divided into at least three stages, and the addition rates of the metal mixed salt solution, the precipitant solution and the complexing agent solution are synchronously increased or decreased in sequence from the previous stage to the next stage, thereby achieving size control of the large-particle positive electrode material precursor, and obtaining a large-particle positive electrode material precursor with uniform particle size distribution and a single-peak distribution in the particle size distribution diagram; therefore, the battery prepared with the obtained large-particle positive electrode material precursor exhibits excellent electrochemical performance;

[0061] (2) In the present invention, by controlling the addition of antioxidants, the oxidation of the metal mixed salt solution is effectively inhibited, thereby improving the structural stability and compaction density of the obtained large-particle positive electrode material precursor, so that the battery prepared with the large-particle positive electrode material precursor exhibits better electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1 This is a particle size distribution diagram of the large-particle positive electrode material precursor provided in Example 1.

[0063] Figure 2 This is a particle size distribution diagram of the large-particle positive electrode material precursor provided in Example 4. DETAILED DESCRIPTION

[0064] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0065] Example 1

[0066] This embodiment provides a method for preparing a large-particle positive electrode material precursor, the preparation method comprising:

[0067] In a nitrogen atmosphere, a nickel-cobalt-manganese mixed salt solution with a total metal ion concentration of 2.5 mol / L (the molar ratio of nickel, cobalt and manganese is 8:1:1), a sodium hydroxide solution with a concentration of 32 wt% and an ammonia solution with a concentration of 0.3 mol / L are mixed into a reaction base liquid with a temperature of 50° C. and a pH of 11, and the mixing is carried out in a first stage, a second stage and a third stage;

[0068] Phase 1:

[0069] The hourly feed rate of the nickel-cobalt-manganese mixed salt solution is 3% of the available capacity of the reaction container, the hourly feed rate of the sodium hydroxide solution is 1.2% of the available capacity of the reaction container, and the hourly feed rate of the ammonia water is 0.3% of the available capacity of the reaction container. The process ends when the particle size distribution diagram of the precipitate changes from multi-peak to single-peak;

[0070] The nickel-cobalt-manganese mixed salt solution, the sodium hydroxide solution and the ammonia water are added while being stirred at a speed of 800 rpm, and the added nickel-cobalt-manganese mixed salt solution also includes ascorbic acid at a concentration of 0.2 g / L;

[0071] Phase 2:

[0072] The addition rate of the nickel-cobalt-manganese mixed salt solution, the sodium hydroxide solution and the ammonia water is 0.7 times that of the first stage. In the second stage, the D50 particle size of the precipitate is tested every hour, and the test ends when the D50 particle size of the precipitate increases by 0.25 μm compared with the D50 particle size of the last sampling test;

[0073] The nickel-cobalt-manganese mixed salt solution, the sodium hydroxide solution and the ammonia water are added while being stirred at a speed of 700 rpm, and the added nickel-cobalt-manganese mixed salt solution also includes ascorbic acid at a concentration of 0.3 g / L;

[0074] Phase 3:

[0075] The addition rate of the mixed salt solution, the precipitant solution and the complexing agent solution is 0.5 times that of the second stage. After the third stage, a large-particle positive electrode material precursor with a D50 particle size of 12 μm is obtained;

[0076] The nickel-cobalt-manganese mixed salt solution, the sodium hydroxide solution and the ammonia water are added while being stirred at a speed of 500 rpm. The added nickel-cobalt-manganese mixed salt solution also includes ascorbic acid at a concentration of 0.5 g / L.

[0077] Example 2

[0078] This embodiment provides a method for preparing a large-particle positive electrode material precursor, the preparation method comprising:

[0079] In an argon atmosphere, a nickel-cobalt-manganese mixed salt solution with a total metal ion concentration of 2 mol / L (the molar ratio of nickel, cobalt and manganese is 8:1:1), a sodium hydroxide solution with a concentration of 30 wt% and an ammonia solution with a concentration of 0.1 mol / L are mixed into a reaction base liquid with a temperature of 40° C. and a pH of 12, and the mixing is carried out in a first stage, a second stage and a third stage;

[0080] Phase 1:

[0081] The hourly feed rate of the nickel-cobalt-manganese mixed salt solution is 4% of the available capacity of the reaction container, the hourly feed rate of the sodium hydroxide solution is 2% of the available capacity of the reaction container, and the hourly feed rate of the ammonia water is 0.5% of the available capacity of the reaction container. The process ends when the particle size distribution diagram of the precipitate changes from multi-peak to single-peak.

[0082] The nickel-cobalt-manganese mixed salt solution, the sodium hydroxide solution and the ammonia water are added while being stirred at a speed of 1000 rpm, and the added nickel-cobalt-manganese mixed salt solution also includes ascorbic acid at a concentration of 0.3 g / L;

[0083] Phase 2:

[0084] The addition rate of the nickel-cobalt-manganese mixed salt solution, the sodium hydroxide solution and the ammonia water is 0.5 times that of the first stage. In the second stage, the D50 particle size of the precipitate is tested every hour, and the test ends when the D50 particle size of the precipitate increases by 0.3 μm compared with the D50 particle size of the last sampling test;

[0085] The nickel-cobalt-manganese mixed salt solution, the sodium hydroxide solution and the ammonia water are added while being stirred at a speed of 600 rpm, and the added nickel-cobalt-manganese mixed salt solution also includes ascorbic acid at a concentration of 0.1 g / L;

[0086] Phase 3:

[0087] The addition rate of the nickel-cobalt-manganese mixed salt solution, the sodium hydroxide solution and the ammonia water is 0.9 times that of the second stage. After the third stage, a large-particle positive electrode material precursor with a D50 particle size of 15 μm is obtained;

[0088] The nickel-cobalt-manganese mixed salt solution, sodium hydroxide solution and ammonia water were added while being stirred at a speed of 600 rpm, and the added metal mixed solution also included ascorbic acid at a concentration of 0.1 g / L.

[0089] Example 3

[0090] This embodiment provides a method for preparing a large-particle positive electrode material precursor, the preparation method comprising:

[0091] In a nitrogen atmosphere, a nickel-cobalt-manganese mixed salt solution with a total metal ion concentration of 3 mol / L (the molar ratio of nickel, cobalt and manganese is 8:1:1), a sodium hydroxide solution with a concentration of 35 wt% and an ammonia solution with a concentration of 0.5 mol / L are mixed into a reaction base liquid with a temperature of 60° C. and a pH of 10, and the mixing is carried out in a first stage, a second stage and a third stage;

[0092] Phase 1:

[0093] The hourly feed rate of the nickel-cobalt-manganese mixed salt solution is 2% of the available capacity of the reaction container, the hourly feed rate of the sodium hydroxide solution is 0.5% of the available capacity of the reaction container, and the hourly feed rate of the ammonia water is 0.1% of the available capacity of the reaction container. The process ends when the particle size distribution diagram of the precipitate changes from multi-peak to single-peak;

[0094] The nickel-cobalt-manganese mixed salt solution, the sodium hydroxide solution and the ammonia water are added while being stirred at a speed of 600 rpm, and the added nickel-cobalt-manganese mixed salt solution also includes ascorbic acid at a concentration of 0.1 g / L;

[0095] Phase 2:

[0096] The addition rate of the nickel-cobalt-manganese mixed salt solution, the sodium hydroxide solution and the ammonia water is 0.9 times that of the first stage. In the second stage, the D50 particle size of the precipitate is tested every hour, and the test ends when the D50 particle size of the precipitate increases by 0.2 μm compared with the D50 particle size of the last sampling test;

[0097] The nickel-cobalt-manganese mixed salt solution, the sodium hydroxide solution and the ammonia water are added while being stirred at a speed of 800 rpm, and the added nickel-cobalt-manganese mixed salt solution also includes ascorbic acid at a concentration of 0.5 g / L;

[0098] Phase 3:

[0099] The addition rate of the nickel-cobalt-manganese mixed salt solution, the sodium hydroxide solution and the ammonia water is 0.1 times that of the second stage. After the third stage, a large-particle positive electrode material precursor with a D50 particle size of 10 μm is obtained;

[0100] The nickel-cobalt-manganese mixed salt solution, the sodium hydroxide solution and the ammonia water are added while being stirred at a speed of 400 rpm. The added nickel-cobalt-manganese mixed salt solution also includes ascorbic acid at a concentration of 1 g / L.

[0101] Example 4

[0102] This embodiment provides a method for preparing a large-particle positive electrode material precursor, the preparation method comprising:

[0103] In an argon atmosphere, a nickel-cobalt-manganese mixed salt solution with a total metal ion concentration of 2.5 mol / L (the molar ratio of nickel, cobalt and manganese is 8:1:1), a potassium hydroxide solution with a concentration of 32 wt% and an oxalic acid solution with a concentration of 0.3 mol / L are mixed into a reaction base liquid with a temperature of 50° C. and a pH of 11, and the mixing is carried out in a first stage, a second stage and a third stage;

[0104] Phase 1:

[0105] The hourly feed rate of the nickel-cobalt-manganese mixed salt solution is 3% of the available capacity of the reaction container, the hourly feed rate of the potassium hydroxide solution is 1.2% of the available capacity of the reaction container, and the hourly feed rate of the oxalic acid solution is 0.3% of the available capacity of the reaction container. The process ends when the particle size distribution diagram of the precipitate changes from multi-peak to single-peak.

[0106] The nickel-cobalt-manganese mixed salt solution, potassium hydroxide solution and oxalic acid solution are added while being stirred at a speed of 800 rpm, and the added nickel-cobalt-manganese mixed salt solution also includes ascorbic acid at a concentration of 0.2 g / L;

[0107] Phase 2:

[0108] The addition rate of the nickel-cobalt-manganese mixed salt solution, potassium hydroxide solution and oxalic acid solution is twice that of the first stage. In the second stage, the D50 particle size of the precipitate is tested every hour, and the test ends when the D50 particle size of the precipitate increases by 0.25 μm compared with the D50 particle size of the last sampling test;

[0109] The nickel-cobalt-manganese mixed salt solution, potassium hydroxide solution and oxalic acid solution were added while being stirred at a speed of 700 rpm, and the added nickel-cobalt-manganese mixed salt solution also included ascorbic acid at a concentration of 0.3 g / L;

[0110] Phase 3:

[0111] The addition rate of the nickel-cobalt-manganese mixed salt solution, the potassium hydroxide solution and the oxalic acid solution is three times that of the second stage. After the third stage, a large-particle positive electrode material precursor with a D50 particle size of 12 μm is obtained;

[0112] The nickel-cobalt-manganese mixed salt solution, potassium hydroxide solution and oxalic acid solution are added while being stirred at a speed of 400-600 rpm, and the added nickel-cobalt-manganese mixed salt solution also includes ascorbic acid at a concentration of 0.1-1 g / L.

[0113] Example 5

[0114] This embodiment provides a method for preparing a large-particle positive electrode material precursor, the preparation method comprising:

[0115] In a nitrogen atmosphere, a nickel-cobalt-manganese mixed salt solution with a total metal ion concentration of 2 mol / L (the molar ratio of nickel, cobalt and manganese is 8:1:1), a potassium hydroxide solution with a concentration of 30 wt% and an ammonia solution with a concentration of 0.1 mol / L are mixed into a reaction base liquid with a temperature of 40° C. and a pH of 12, and the mixing is carried out in a first stage, a second stage and a third stage;

[0116] Phase 1:

[0117] The hourly feed rate of the nickel-cobalt-manganese mixed salt solution is 4% of the available capacity of the reaction container, the hourly feed rate of the potassium hydroxide solution is 2% of the available capacity of the reaction container, and the hourly feed rate of the ammonia water is 0.5% of the available capacity of the reaction container. The process ends when the particle size distribution diagram of the precipitate changes from multi-peak to single-peak.

[0118] The nickel-cobalt-manganese mixed salt solution, potassium hydroxide solution and ammonia water are added while being stirred at a speed of 1000 rpm, and the added nickel-cobalt-manganese mixed salt solution also includes ascorbic acid at a concentration of 0.3 g / L;

[0119] Phase 2:

[0120] The addition rate of the nickel-cobalt-manganese mixed salt solution, potassium hydroxide solution and ammonia water is 1.1 times that of the first stage. In the second stage, the D50 particle size of the precipitate is tested every hour, and the test ends when the D50 particle size of the precipitate increases by 0.3 μm compared with the D50 particle size of the last sampling test;

[0121] The nickel-cobalt-manganese mixed salt solution, potassium hydroxide solution and ammonia water are added while being stirred at a speed of 600 to 800 rpm, and the added nickel-cobalt-manganese mixed salt solution also includes ascorbic acid at a concentration of 0.1 g / L;

[0122] Phase 3:

[0123] The addition rate of the nickel-cobalt-manganese mixed salt solution, potassium hydroxide solution and ammonia water is 5.5 times that of the second stage. After the third stage, a large-particle positive electrode material precursor with a D50 particle size of 15 μm is obtained;

[0124] The nickel-cobalt-manganese mixed salt solution, potassium hydroxide solution and ammonia water were added while being stirred at a speed of 600 rpm. The added nickel-cobalt-manganese mixed salt solution also included ascorbic acid at a concentration of 0.1 g / L.

[0125] Example 6

[0126] This embodiment provides a method for preparing a large-particle positive electrode material precursor, which is the same as that of Embodiment 1 except that the method stops when the particle size distribution diagram of the precipitate suddenly changes from multi-peaks to bi-peaks in the first stage.

[0127] Example 7

[0128] This embodiment provides a method for preparing a large-particle positive electrode material precursor, which is the same as that of Embodiment 4 except that the method stops when the particle size distribution diagram of the precipitate suddenly changes from multi-peaks to bi-peaks in the first stage.

[0129] Example 8

[0130] This embodiment provides a method for preparing a large-particle positive electrode material precursor, which is the same as Example 1 except that the addition rate of the nickel-cobalt-manganese mixed salt solution, sodium hydroxide solution and ammonia water in the second stage is 0.3 times that of the first stage.

[0131] Example 9

[0132] This embodiment provides a method for preparing a large-particle positive electrode material precursor, which is the same as Example 1 except that the addition rate of the nickel-cobalt-manganese mixed salt solution, sodium hydroxide solution and ammonia water in the second stage is 0.95 times that of the first stage.

[0133] Example 10

[0134] This embodiment provides a method for preparing a large-particle positive electrode material precursor, which is the same as Example 4 except that the addition rate of the nickel-cobalt-manganese mixed salt solution, potassium hydroxide solution and oxalic acid solution in the second stage is 1.05 times that of the first stage.

[0135] Embodiment 11

[0136] This embodiment provides a method for preparing a large-particle positive electrode material precursor, which is the same as Example 4 except that the addition rate of the nickel-cobalt-manganese mixed salt solution, potassium hydroxide solution and oxalic acid solution in the second stage is 3.8 times that of the first stage.

[0137] Example 12

[0138] This embodiment provides a method for preparing a large-particle positive electrode material precursor, which is the same as that of Embodiment 1 except that the second stage is terminated when the D50 particle size of the precipitate increases by 0.18 μm compared with the D50 particle size of the last sampling test.

[0139] Embodiment 13

[0140] This embodiment provides a method for preparing a large-particle positive electrode material precursor, which is the same as that of Example 4 except that in the second stage, the method ends when the D50 particle size of the precipitate increases by 0.18 μm compared with the D50 particle size of the previous sampling test.

[0141] Embodiment 14

[0142] This embodiment provides a method for preparing a large-particle positive electrode material precursor, which is the same as Example 1 except that the addition rate of the nickel-cobalt-manganese mixed salt solution, sodium hydroxide solution and ammonia water in the third stage is 0.05 times that of the second stage.

[0143] Embodiment 15

[0144] This embodiment provides a method for preparing a large-particle positive electrode material precursor, which is the same as Example 1 except that the addition rate of the nickel-cobalt-manganese mixed salt solution, sodium hydroxide solution and ammonia water in the third stage is 0.95 times that of the second stage.

[0145] Example 16

[0146] This embodiment provides a method for preparing a large-particle positive electrode material precursor, which is the same as Example 4 except that the addition rate of the nickel-cobalt-manganese mixed salt solution, potassium hydroxide solution and oxalic acid solution in the third stage is 1.05 times that of the second stage.

[0147] Embodiment 17

[0148] This embodiment provides a method for preparing a large-particle positive electrode material precursor, which is the same as Example 4 except that the addition rate of the nickel-cobalt-manganese mixed salt solution, potassium hydroxide solution and oxalic acid solution in the third stage is 6 times that of the second stage.

[0149] Comparative Example 1

[0150] This comparative example provides a method for preparing a large-particle positive electrode material precursor, which is the same as Example 1 except that the mixing is divided into two stages, that is, the first stage is omitted.

[0151] Comparative Example 2

[0152] This comparative example provides a method for preparing a large-particle positive electrode material precursor, which is the same as Example 4 except that the mixing is divided into two stages, that is, the first stage is omitted.

[0153] Comparative Example 3

[0154] This comparative example provides a method for preparing a large-particle positive electrode material precursor, which is the same as Example 1 except that the mixing is divided into two stages, that is, the second stage is omitted.

[0155] Comparative Example 4

[0156] This comparative example provides a method for preparing a large-particle positive electrode material precursor, which is the same as Example 4 except that the mixing is divided into two stages, that is, the second stage is omitted.

[0157] Comparative Example 5

[0158] This comparative example provides a method for preparing a large-particle positive electrode material precursor, which is the same as Example 1 except that the addition rate of the nickel-cobalt-manganese mixed salt solution, sodium hydroxide solution and ammonia water in the second stage is 1.1 times that of the first stage.

[0159] Comparative Example 6

[0160] This comparative example provides a method for preparing a large-particle positive electrode material precursor, which is the same as Example 4 except that the addition rate of the nickel-cobalt-manganese mixed salt solution, potassium hydroxide solution and oxalic acid solution in the second stage is 0.9 times that of the first stage.

[0161] The tap density and specific surface area of ​​the large-particle positive electrode material precursors obtained in the above examples and comparative examples were tested, and the test results are shown in Table 1;

[0162] The large-particle cathode material precursors obtained in the above examples and comparative examples were subjected to Malvern particle size test, and the standard deviation of the particle size distribution and the number of peaks in the particle size distribution diagram obtained by the test are shown in Table 1; wherein the particle size distribution diagram of the large-particle cathode material precursor provided in Example 1 is shown in Figure 1 As shown, the particle size distribution diagram of the large particle positive electrode material precursor provided in Example 4 is as follows Figure 2 As shown;

[0163] The large-particle positive electrode material precursor obtained in the above embodiment and comparative example is used to prepare the large-particle positive electrode material. The method for preparing the large-particle positive electrode material is as follows: mixing the obtained large-particle positive electrode material precursor with a lithium hydroxide solution having a mass concentration of 30wt%, stirring for 8h under a nitrogen atmosphere, washing and drying, and sintering at 1000°C to obtain the positive electrode material;

[0164] A battery is prepared with the obtained large-particle positive electrode material, and the method for preparing the battery is: preparing the obtained battery positive electrode material into a positive electrode sheet, and then using a metal lithium sheet as a negative electrode, and NaClO4 solution or LiPF6 as an electrolyte to assemble into a button battery; the first efficiency, cycle performance and rate performance of the obtained button battery are tested, and the method is: charging and discharging at 0.1C / 0.1C in a voltage window of 2.0V-4.0V is used to perform a charge and discharge test to obtain the first discharge specific capacity, the capacity retention rate after 100 cycles and the 2C rate performance. The test results are shown in Table 2.

[0165] Table 1

[0166]

[0167]

[0168] Table 2

[0169]

[0170]

[0171] From Table 1 and Table 2, we can get:

[0172] (1) The large-particle positive electrode material precursor prepared by the preparation method of the large-particle positive electrode material precursor provided in Examples 1 to 5 exhibits a higher tap density, and the standard deviation of the particle size distribution obtained in the Malvern particle size test is small, and the particle size distribution diagram presents a single peak distribution; at the same time, the battery prepared by the obtained large-particle positive electrode material precursor exhibits a higher first efficiency, excellent cycle stability and strong rate performance;

[0173] (2) By comparing Example 1 with Examples 6 and 7, it can be seen that the number of peaks in the particle size distribution diagram of the precipitate when the first stage is stopped will affect the parameters of the large-particle positive electrode material precursor and the performance of the prepared battery; when the number of peaks in the particle size distribution diagram of the precipitate when the first stage is stopped is greater than one, it will lead to a lower tap density, a larger specific surface area, a larger standard deviation, and an increase in the number of peaks, which will lead to a lower first efficiency of the battery, a lower capacity retention rate, and a lower rate performance. This is because small particles are continuously generated, resulting in uneven precursor particle size;

[0174] (3) By comparing Example 1 with Examples 8 and 9, it can be seen that when the addition speeds of the mixed salt solution, the precipitant solution and the complexing agent solution in the first stage, the second stage and the third stage are synchronously decreased in sequence, the multiple of the addition speed in the second stage relative to the first stage will affect the parameters of the large-particle positive electrode material precursor and the performance of the prepared battery; when the multiple of the addition speed in the second stage relative to the first stage is too small, it will cause the tap density to become lower, the specific surface area to become larger, the standard deviation to become larger, and the number of peaks to become more, which will cause the first efficiency of the battery to become lower, the capacity retention rate to become lower, and the rate performance to become lower. This is because the flow rate of the metal salt solution is too low, which makes it difficult for small particles to grow; when the multiple of the addition speed in the second stage relative to the first stage is too large, it will cause the tap density to become lower, the specific surface area to become larger, the standard deviation to become larger, and the number of peaks to become more, which will cause the first efficiency of the battery to become lower, the capacity retention rate to become lower, and the rate performance to become lower. This is because the flow rate of the metal salt solution is too fast, resulting in the generation of small particles;

[0175] (4) By comparing Example 1 with Examples 10 and 11, it can be seen that when the addition speeds of the mixed salt solution, the precipitant solution and the complexing agent solution in the first stage, the second stage and the third stage are synchronously increased in sequence, the multiple of the addition speed in the second stage relative to the first stage will affect the parameters of the large-particle positive electrode material precursor and the performance of the prepared battery; when the multiple of the addition speed in the second stage relative to the first stage is too small, it will cause the tap density to become lower, the specific surface area to become larger, the standard deviation to become larger, and the number of peaks to become more, which will cause the first efficiency of the battery to become lower, the capacity retention rate to become lower, and the rate performance to become lower. This is because the flow rate of the metal salt solution is too low, which makes it difficult for small particles to grow; when the multiple of the addition speed in the second stage relative to the first stage is too large, it will cause the tap density to become lower, the specific surface area to become larger, the standard deviation to become larger, and the number of peaks to become more, which will cause the first efficiency of the battery to become lower, the capacity retention rate to become lower, and the rate performance to become lower. This is because the flow rate of the metal salt solution is too fast, resulting in the generation of small particles;

[0176] (5) By comparing Example 1 with Examples 12 and 13, it can be seen that in the second stage of the present invention, when the D50 particle size of the precipitate increases by less than 0.2 μm compared with the D50 particle size of the previous sampling test, the tap density will be lower, the specific surface area will be larger, the standard deviation will be larger, the number of peaks will be more, and the first efficiency of the battery will be lower, the capacity retention rate will be lower, and the rate performance will be lower. This is because the flow rate of the metal salt solution is too low, which makes it difficult for small particles to grow;

[0177] (6) By comparing Example 1 with Examples 14 and 15, it can be seen that when the addition speeds of the mixed salt solution, the precipitant solution and the complexing agent solution in the first stage, the second stage and the third stage are synchronously decreased in sequence, the multiple of the addition speed in the third stage relative to the second stage will affect the parameters of the large-particle positive electrode material precursor and the performance of the prepared battery; when the multiple of the addition speed in the third stage relative to the second stage is too small, it will cause the tap density to become lower, the specific surface area to become larger, the standard deviation to become larger, and the number of peaks to become more, which will cause the first efficiency of the battery to become lower, the capacity retention rate to become lower, and the rate performance to become lower. This is because the flow rate of the metal salt solution is too low, making it difficult for small particles to grow; when the multiple of the addition speed in the third stage relative to the second stage is too large, it will cause the tap density to become lower, the specific surface area to become larger, the standard deviation to become larger, and the number of peaks to become more, which will cause the first efficiency of the battery to become lower, the capacity retention rate to become lower, and the rate performance to become lower. This is because the flow rate of the metal salt solution is too fast, resulting in the generation of small particles;

[0178] (7) By comparing Example 1 with Examples 16 and 17, it can be seen that when the addition speeds of the mixed salt solution, the precipitant solution and the complexing agent solution in the first stage, the second stage and the third stage are synchronously increased in sequence, the multiple of the addition speed in the third stage relative to the second stage will affect the parameters of the large-particle positive electrode material precursor and the performance of the prepared battery; when the multiple of the addition speed in the third stage relative to the second stage is too small, it will cause the tap density to become lower, the specific surface area to become larger, the standard deviation to become larger, and the number of peaks to become more, which will cause the first efficiency of the battery to become lower, the capacity retention rate to become lower, and the rate performance to become lower. This is because the flow rate of the metal salt solution is too low, which makes it difficult for small particles to grow; when the multiple of the addition speed in the third stage relative to the second stage is too large, it will cause the tap density to become lower, the specific surface area to become larger, the standard deviation to become larger, and the number of peaks to become more, which will cause the first efficiency of the battery to become lower, the capacity retention rate to become lower, and the rate performance to become lower. This is because the flow rate of the metal salt solution is too fast, resulting in the generation of small particles;

[0179] (8) By comparing Example 1 with Comparative Examples 1 to 6, it can be seen that the mixing process in the present invention is divided into at least three stages, and after the previous stage to the next stage, the addition speed of the metal mixed salt solution, the precipitant solution and the complexing agent solution is synchronously increased or decreased in sequence, thereby achieving size control of the large-particle positive electrode material precursor, and obtaining a large-particle positive electrode material precursor with uniform particle size distribution and a particle size distribution diagram showing a single peak distribution; therefore, the battery prepared with the obtained large-particle positive electrode material precursor exhibits excellent electrochemical performance.

[0180] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a large-particle positive electrode material precursor, characterized in that: The preparation method comprises: In a protective atmosphere, a metal mixed salt solution, a precipitant solution and a complexing agent solution are mixed into a reaction base liquid to obtain a large-particle positive electrode material precursor; The mixing is carried out in at least three stages. Each time after entering the next stage from the previous stage, the adding speed of the metal mixed salt solution, the precipitant solution and the complexing agent solution is synchronously increased or decreased in sequence.

2. The preparation method according to claim 1, characterized in that: The mixing is divided into a first stage, a second stage and a third stage, and the adding speeds of the mixed salt solution, the precipitant solution and the complexing agent solution in the first stage, the second stage and the third stage are synchronously decreased or increased in sequence.

3. The preparation method according to claim 2, characterized in that: The addition rates of the mixed salt solution, the precipitant solution and the complexing agent solution in the first stage, the second stage and the third stage are synchronously decreased in sequence; Preferably, in the first stage, the feed rate of the mixed salt solution per hour is 2-4% of the available capacity of the reaction container, the feed rate of the precipitant solution per hour is 0.5-2% of the available capacity of the reaction container, and the feed rate of the complexing agent solution per hour is 0.1-0.5% of the available capacity of the reaction container; Preferably, the first stage ends when the particle size distribution diagram of the precipitate changes from multi-peak to single peak; Preferably, the addition rates of the mixed salt solution, the precipitant solution and the complexing agent solution in the second stage are independently 0.5 to 0.9 times that of the first stage; Preferably, the D50 particle size of the precipitate is tested every hour in the second stage, and the test ends when the D50 particle size of the precipitate increases by no less than 0.2 μm compared with the D50 particle size of the last sampling test; Preferably, the addition rates of the mixed salt solution, the precipitant solution and the complexing agent solution in the third stage are independently 0.1 to 0.9 times that of the second stage.

4. The preparation method according to claim 2, characterized in that: The addition rates of the mixed salt solution, the precipitant solution and the complexing agent solution in the first stage, the second stage and the third stage are increased synchronously and successively; Preferably, in the first stage, the feed rate of the mixed salt solution per hour is 2-4% of the available capacity of the reaction container, the feed rate of the precipitant solution per hour is 0.5-2% of the available capacity of the reaction container, and the feed rate of the complexing agent solution per hour is 0.1%-0.5% of the available capacity of the reaction container; Preferably, the first stage ends when the particle size distribution diagram of the precipitate changes from multi-peak to single peak; Preferably, the addition rates of the mixed salt solution, the precipitant solution and the complexing agent solution in the second stage are independently 1.1 to 3.5 times that of the first stage; Preferably, the D50 particle size of the precipitate is tested every hour in the second stage, and the test ends when the D50 particle size of the precipitate increases by no less than 0.2 μm compared with the D50 particle size of the last sampling test; Preferably, the addition rate of the mixed salt solution, the precipitant solution and the complexing agent solution in the third stage is 1.1 to 5.5 times that of the second stage, respectively.

5. The preparation method according to any one of claims 2 to 4, characterized in that: The metal mixture solution in the first stage also includes an antioxidant with a concentration of 0.1 to 0.3 g / L; Preferably, the addition of the metal mixed salt solution, the precipitant solution and the complexing agent solution in the first stage is accompanied by stirring at a speed of 600 to 1000 rpm; Preferably, the metal mixture solution in the second stage further includes an antioxidant at a concentration of 0.1 to 0.5 g / L; Preferably, the addition of the metal mixed salt solution, the precipitant solution and the complexing agent solution in the second stage is accompanied by stirring at a speed of 600 to 800 rpm; Preferably, the metal mixed solution in the third stage further includes an antioxidant with a concentration of 0.1 to 1 g / L; Preferably, the addition of the metal mixed salt solution, the precipitant solution and the complexing agent solution in the third stage is accompanied by stirring at a rotation speed of 400 to 600 rpm.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The reaction base liquid includes a solvent, a precipitant and a complexing agent, and the temperature of the reaction base liquid is 40-60° C. and the pH is 10-12; Preferably, during the entire mixing process, the pH of the mixed solution of the reaction base solution, the metal mixed salt solution, the precipitant solution and the complexing agent solution is controlled to be 9.5 to 10.8; Preferably, the total concentration of metal ions in the metal mixed salt solution is 2 to 3 mol / L; Preferably, the mass concentration of the precipitant in the precipitant solution is 30-35wt%; Preferably, the concentration of the complexing agent in the complexing agent solution is 0.1-0.5 mol / L.

7. A large-particle cathode material precursor, characterized in that: The large-particle positive electrode material precursor is obtained by the preparation method described in any one of claims 1 to 6.

8. The large-particle positive electrode material precursor according to claim 7, characterized in that: The D50 particle size of the large-particle positive electrode material precursor is 10 to 15 μm; Preferably, the specific surface area of ​​the large-particle positive electrode material precursor is 9 to 15 m 2 / g; Preferably, the tap density of the large-particle positive electrode material precursor is 1.5 to 2.5 g / cm 3 .

9. A large-particle positive electrode material, characterized in that: The large-particle positive electrode material is prepared from the large-particle positive electrode material precursor according to claim 7 or 8.

10. A battery, characterized in that: The battery comprises the large-particle positive electrode material according to claim 9.

Citation Information

Cited By

  • Ultrahigh-nickel ternary precursor and preparation method thereof, positive electrode material, lithium ion battery and electric equipment

    CN120483291A

  • An ultrahigh-nickel ternary precursor, a preparation method thereof, a positive electrode material, a lithium ion battery, and an electric device

    CN120483291B