Micro reaction channel and micro reactor
By forming a catalyst coating with a microporous structure on the inner wall of the microreaction channel, the problem of low efficiency of multi-phase catalytic reactions under high temperature and high pressure is solved, achieving efficient reactions without reloading the catalyst and reducing costs.
Patent Information
- Application Number
- CN202410954466.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-17
AI Technical Summary
Existing microreactors are unable to carry out heterogeneous catalytic reactions under high temperature (200-400°C) and high pressure (5-30MPa) conditions. In particular, the catalyst loading is inconvenient, resulting in low reaction efficiency.
A coating is formed on the inner wall of the microreaction channel. Through the preparation and solidification of the catalyst precursor and the epoxy resin, a catalyst coating with a microporous structure is formed, which avoids the refilling of the catalyst and realizes heterogeneous catalytic reactions under high temperature and pressure. .
It achieves a stable heterogeneous catalytic reaction under high temperature and pressure, improves reaction efficiency, reduces costs, and significantly improves the durability and catalytic performance of the coating.
Smart Images

Figure CN118491440B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of microreactor equipment, in particular to a microreaction channel and a microreactor. Background Art
[0002] A microreactor is a device that performs chemical reactions at a microscopic scale. It is usually composed of microchannels, mixers, separators, and control units. Its development background can be traced back to the early 1990s, when the rise of microfluidics provided a technical basis for the development of microreactors. With the continuous advancement of micromachining technology and microfluidics technology, microreactors have gradually become a research hotspot in the fields of chemical synthesis, biomedicine, and materials science. Its characteristics include miniaturization, efficient mixing, rapid heat and mass transfer, and precise control. Its advantages lie in reducing the amount of reaction materials used, increasing reaction rates and product purity, and achieving precise control of reaction conditions.
[0003] However, the disadvantages may include high requirements for manufacturing and operating technology, high requirements for the purity and stability of the reaction materials, and some reactions are not suitable for being carried out in a microreactor. At present, there is a Chinese utility model patent CN211586541U that discloses a microreactor, wherein there is a microchannel inside the microreactor, and the channel has a liquid inlet and a liquid outlet. There is a containing layer made of porous material on the bottom wall, which can accommodate solid particles generated by the reaction to prevent channel blockage and solid particles from mixing into the fluid. For reactions requiring a catalyst, the catalyst can be placed in the containing layer in advance to increase the reaction rate. However, the pores in the microreactor prepared by this method have the characteristics of one end open and the other end closed. When the reaction proceeds to a certain time, the particles will block the pores, causing the reaction to be unable to proceed. Chinese utility model patent CN208975763U discloses a multi-channel microreactor for synthesizing poly-alpha-olefin synthetic oil, including a distribution chamber, a reaction heat exchange zone and a collection chamber. The distribution chamber is provided with a distribution component, the reaction heat exchange zone is composed of a plurality of reaction channels and adjacent heat exchange channels, and a mixing component is provided in the reaction channel. The inlet of the microreactor is connected in sequence through the distribution chamber, the reaction channel, the collection chamber and the outlet of the microreactor, and the inlet of the heat exchange medium is connected to the outlet of the heat exchange medium through the heat exchange channel. The reactor can maintain the stability of the reaction heat exchange, strengthen the reaction process, improve the conversion rate, and shorten the reaction time. However, the device does not involve the use and loading of the catalyst and is only applicable to homogeneous catalytic reactions or non-catalytic reactions.
[0004] The above-mentioned microreactors are all unable to carry out heterogeneous catalytic reactions under high temperature (200-400° C.), high pressure (5-30 MPa) and hydrothermal conditions. Summary of the invention
[0005] In order to solve the above technical problems, the embodiments of the present invention provide a micro-reaction channel and a micro-reactor to realize a multi-phase catalytic reaction and avoid the need to load catalysts during the reaction.
[0006] To achieve the above object, the embodiments of the present invention adopt the following technical solutions:
[0007] In one aspect, the present invention provides a micro-reaction channel, comprising a coating attached to the inner wall of the micro-reaction channel, wherein the method for preparing the coating comprises the following steps:
[0008] A. The catalyst precursor and epoxy resin are prepared into a glue solution, and the glue solution is evenly distributed on the inner wall of the micro-reaction channel to form a coating;
[0009] B. preparing a displacement liquid with solid particles, a polymer matrix dispersant and a dispersion medium, and cleaning the micro-reaction channel with the displacement liquid to wash out the residual catalyst precursor and epoxy resin, and then cleaning with clean water;
[0010] C. Under a nitrogen protective atmosphere, the micro-reaction channel cleaned in step B is placed in a tube furnace to cure the coating so that the coating forms a microporous structure.
[0011] In some embodiments, in step A, the mass ratio of the catalyst precursor to the epoxy resin is 1-5%.
[0012] In some embodiments, in step A, the catalyst precursor includes at least one of ferric nitrate nonahydrate, nickel nitrate hexahydrate, iron naphthenate, cobalt stearate, manganese laurate, nickel stearate, copper laurate, zinc oleate, cobalt laurate, cobalt nitrate and zinc nitrate.
[0013] In some embodiments, in step A, the epoxy resin includes at least one of epoxy silicone resin, phosphorus-containing epoxy resin, carbon nanotube-reinforced epoxy resin, and aluminum-containing epoxy resin.
[0014] In some embodiments, in step A, the coating has a thickness of 1 to 100 μm.
[0015] In some embodiments, in step B, based on the percentage of the total weight of the raw materials, the solid particles are 20-40%, the polymer matrix dispersant is 0.5-1%, and the dispersion medium is 50-98%.
[0016] In some embodiments, in step B, the solid particles include at least one of silicon dioxide, corundum and silicon carbide, the particle size of the solid particles is 20 to 500 nm, the polymer matrix dispersant includes at least one of polyacrylamide, polyvinyl alcohol and sodium polyacrylate, and the dispersion medium is water.
[0017] In some embodiments, in step C, the coating is cured in the tube furnace to form a microporous structure of the coating, specifically comprising the following steps: nitrogen is introduced as a protective gas at an air velocity of 1 to 10 h -1, heat up to 40-80°C at a heating rate of 5-50°C / min, dry for 6-12h, then heat up to 90-120°C at a heating rate of 5-50°C / min, keep for 1-6h, solidify the coating evenly distributed on the inner wall of the microreaction channel, then continue to heat up to 200°C at a heating rate of 5-10°C / min, and then continue to heat up to 300-450°C at a heating rate of 10-20°C / min, and keep for 2-6h.
[0018] In some embodiments, in step C, the porosity of the coating is 10-50%, and the size of the micropores is 10-500 nm.
[0019] On the other hand, the present invention also provides a microreactor, comprising a steam pipeline, a storage tank, a collecting tank, a microreaction channel, a reactant input pipe and a distributor. The steam pipeline is used to pass steam. The storage tank is installed in the steam pipeline. The collecting tank has a reactant outlet, and the collecting tank is installed in the steam pipeline. The microreaction channel is installed between the storage tank and the collecting tank and is connected thereto. One end of the reactant input pipe is connected to the storage tank, and the other end extends outward through the steam pipeline. The distributor is installed in the storage tank and is located at a position where the reactant input pipe is connected to the storage tank.
[0020] During the curing process, the catalyst precursor of the coating on the inner wall of the micro-reaction channel of the present invention decomposes to generate gas, which is dispersed on the coating in the gas, thereby forming a microporous structure and a certain roughness on the coating, forming a coating resistant to high temperature, high salt and hydrothermal, and generating a catalyst with catalytic function on its surface and in the pores. The cured catalyst can stably have a catalytic effect on the inner wall of the micro-reaction channel for a long time, thereby accelerating the reaction process under the action of the catalyst, without the need to reload the catalyst into the micro-reaction channel, and integrating multiple micro-reaction channels in parallel to form a microreactor, which can achieve large-scale rapid reaction. The binder in the coating uses cured epoxy resin, which is low in cost, easy to obtain, and resistant to high temperature and high pressure. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Schematic diagram of the microreactor structure of the present invention. DETAILED DESCRIPTION
[0022] The following will be combined with the accompanying drawings to clearly and completely describe the technical solutions in some embodiments of the present disclosure. Obviously, the described embodiments are only part of the embodiments of the present disclosure, rather than all the embodiments. Based on the embodiments provided by the present disclosure, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present disclosure.
[0023] In order to better understand the device of the present invention, the following is the preparation method of the device and the specific implementation process. It should be noted that the entire implementation method is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0024] Example 1
[0025] Ferric nitrate nonahydrate and nickel nitrate hexahydrate are mixed in a metal atomic molar ratio of 1:1 and then mixed with epoxy silicone resin as a catalyst precursor to prepare a glue solution, which is added in a mass ratio of 1% between the catalyst precursor and the epoxy silicone resin, and the glue solution is slowly injected into the microreactor channel so that the glue solution is evenly distributed on the inner wall of the microreactor channel to form a coating with a porosity of 15%. Subsequently, a displacement fluid is used to wash out the remaining catalyst precursor and epoxy silicone resin, and the displacement fluid is composed of silicon dioxide, polyacrylamide and water, and is configured with a mass fraction of 30% silicon dioxide, 0.5% polyacrylamide and 69.5% clean water.
[0026] Then it was cleaned with water for a second time. The cleaned micro-reaction channel was placed in a tubular furnace and nitrogen was introduced as a protective gas. The air velocity was controlled at 5h -1 , heat to 60°C at a heating rate of 10°C / min, dry for 10 hours, then heat to 120°C at a heating rate of 30°C / min, maintain for 3 hours, completely solidify the suspension evenly distributed on the inner wall of the microreaction channel, then continue to heat to 200°C at a heating rate of 10°C / min, and then continue to heat to 450°C at a heating rate of 20°C / min for treatment for 2 hours.
[0027] During the high-temperature calcination process, ferric nitrate nonahydrate and nickel nitrate hexahydrate decompose to generate active components - iron oxide and nickel oxide. The gases produced at the same time will form micropores in the cured epoxy silicone resin coating and form an outer surface with a certain roughness (roughness is Ra12.5) on the surface, ensuring that the catalyst has sufficient reaction specific surface area to react with the reactants.
[0028] The metal oxides (active ingredients) are evenly distributed on the outer surface of the coating and in the micropores. The thickness of the catalyst coating in the microreaction channel is 50 μm, thus preparing a microreaction channel that is resistant to high temperature, high salt and hydrothermal conditions.
[0029] like Figure 1As shown, the microreactor comprises a steam pipe 1, a storage tank 2, a collecting tank 3, a micro-reaction channel 5, a reactant input pipe 6 and a distributor 7. The steam pipe 1 is used to pass steam. The storage tank 2 is installed in the steam pipe 1. The collecting tank 3 has a reactant outlet 4, and the collecting tank 3 is installed in the steam pipe 1. The micro-reaction channel 5 is installed between the storage tank 2 and the collecting tank 3 and is connected thereto. The micro-reaction channel 5 can be ten and have a length of five meters. One end of the reactant input pipe 6 is connected to the storage tank 2, and the other end extends outward through the steam pipe 1. The distributor 7 is installed in the storage tank 2 and is located at the position where the reactant input pipe 6 is connected to the storage tank 2. By passing steam in the steam pipe 1, the reactant enters the distributor 7 and the storage tank 2 through the reactant input pipe 6, and then enters the micro-reaction channel 5 to react. The product after the reaction is in the collecting tank 3 and discharged through the reactant outlet 4.
[0030] Example 2
[0031] Ferric cyclopentaneate is used as a catalyst precursor and mixed with epoxy silicone resin to prepare a glue solution, which is added at a mass ratio of 3% between the catalyst precursor and the epoxy silicone resin. The glue solution is slowly injected into the microreactor channel so that the glue solution is evenly distributed on the inner wall of the microreactor channel to form a coating with a porosity of 30%. Subsequently, a displacement fluid is used to wash out the remaining catalyst precursor and epoxy silicone resin. The displacement fluid is composed of corundum, polyvinyl alcohol and water, and is configured with a mass fraction of 20% silicon dioxide, 0.8% polyvinyl alcohol and 79.2% water.
[0032] Then it was cleaned with water for a second time. The cleaned micro-reaction channel was placed in a tubular furnace and nitrogen was introduced as a protective gas. The air velocity was controlled at 8h -1 , the temperature was raised to 80°C at a rate of 5°C / min, dried for 12 hours, and then raised to 120°C at a rate of 20°C / min, maintained for 2 hours, and the suspension evenly distributed on the inner wall of the micro-reaction channel was completely solidified. Then the temperature was raised to 200°C at a rate of 15°C / min, and then raised to 300°C at a rate of 10°C / min for 3 hours.
[0033] During the high-temperature calcination process, iron alkanoate decomposes to form the active component - iron oxide. The gas produced at the same time will form micropores in the cured epoxy resin coating and form an outer surface with a certain roughness (Ra6.3) on the surface. The active component - iron oxide is evenly distributed on the outer surface of the coating and in the micropores. The thickness of the catalyst coating in the microreaction channel is 80μm, thereby preparing a microreaction channel resistant to high temperature, high salt and hydrothermal.
[0034] like Figure 1As shown, the microreactor comprises a steam pipe 1, a storage tank 2, a collecting tank 3, a micro-reaction channel 5, a reactant input pipe 6 and a distributor 7. The steam pipe 1 is used to pass steam. The storage tank 2 is installed in the steam pipe 1. The collecting tank 3 has a reactant outlet 4, and the collecting tank 3 is installed in the steam pipe 1. The micro-reaction channel 5 is installed between the storage tank 2 and the collecting tank 3 and is connected thereto. The micro-reaction channel 5 can be ten and have a length of eight meters. One end of the reactant input pipe 6 is connected to the storage tank 2, and the other end extends outward through the steam pipe 1. The distributor 7 is installed in the storage tank 2 and is located at the position where the reactant input pipe 6 is connected to the storage tank 2. By passing steam in the steam pipe 1, the reactant enters the distributor 7 and the storage tank 2 through the reactant input pipe 6, and then enters the micro-reaction channel 5 to react. The product after the reaction is in the collecting tank 3 and discharged through the reactant outlet 4.
[0035] Example 3
[0036] The metal atoms in cobalt stearate and manganese laurate are mixed in a molar ratio of 1:2 and then used as a catalyst precursor and mixed with phosphorus-containing epoxy silicone resin to prepare a glue solution, which is added in a mass ratio of 2% of the catalyst precursor to the phosphorus-containing epoxy silicone resin, and the glue solution is slowly injected into the microreactor channel so that the glue solution is evenly distributed on the inner wall of the microreactor channel to form a coating with a porosity of 45%; subsequently, the residual catalyst precursor and phosphorus-containing epoxy resin are washed out with a displacement fluid, which is composed of silicon carbide, sodium polyacrylate and water, and is configured with a mass fraction of 40% silicon dioxide, 1.0% sodium polyacrylate and 59.0% water.
[0037] Then it was cleaned with water for a second time. The cleaned micro-reaction channel was placed in a tubular furnace and nitrogen was introduced as a protective gas. The air velocity was controlled at 10 h -1 , the temperature was raised to 80°C at a heating rate of 20°C / min, dried for 8 hours, and then raised to 100°C at a heating rate of 15°C / min, maintained for 3 hours, and the suspension evenly distributed on the inner wall of the micro-reaction channel was completely solidified. Then the temperature was raised to 200°C at a heating rate of 20°C / min, and then continued to rise to 400°C at a heating rate of 20°C / min for 2.5 hours.
[0038] During the high-temperature calcination process, cobalt stearate and lauric acid violently decompose to form active components - cobalt oxide and manganese oxide. The gases produced at the same time will form micropores in the cured epoxy resin coating and form an outer surface with a certain roughness (Ra3.2) on the surface. The metal oxides are evenly distributed on the outer surface of the coating and in the microchannels. The thickness of the catalyst coating in the microreaction channel is usually 100μm, thereby preparing a microreaction channel that is resistant to high temperature, high salt and hydrothermal conditions.
[0039] like Figure 1 As shown, the microreactor comprises a steam pipe 1, a storage tank 2, a collecting tank 3, a micro-reaction channel 5, a reactant input pipe 6 and a distributor 7. The steam pipe 1 is used to pass steam. The storage tank 2 is installed in the steam pipe 1. The collecting tank 3 has a reactant outlet 4, and the collecting tank 3 is installed in the steam pipe 1. The micro-reaction channel 5 is installed between the storage tank 2 and the collecting tank 3 and is connected thereto. The micro-reaction channel 5 can be eight and six meters long. One end of the reactant input pipe 6 is connected to the storage tank 2, and the other end extends outward through the steam pipe 1. The distributor 7 is installed in the storage tank 2 and is located at the position where the reactant input pipe 6 is connected to the storage tank 2. By passing steam in the steam pipe 1, the reactant enters the distributor 7 and the storage tank 2 through the reactant input pipe 6, and then enters the micro-reaction channel 5 to react. The product after the reaction is in the collecting tank 3 and discharged through the reactant outlet 4.
[0040] Example 4
[0041] Nickel stearate and copper laurate are mixed in a metal molar ratio of 2:1 and then used as a catalyst precursor and mixed with epoxy resin (carbon nanotube enhanced epoxy coating) to prepare a glue solution, which is added in a mass ratio of 5% between the catalyst precursor and the carbon nanotube epoxy resin, and the glue solution is slowly injected into a microreactor channel so that the glue solution is evenly distributed on the inner wall of the microreactor channel to form a coating with a porosity of 40%; subsequently, a displacement fluid is used to wash out the remaining catalyst precursor and carbon nanotube epoxy resin, and the displacement fluid is composed of silicon carbide, polyacrylamide and water, and is configured with a mass fraction of 30% silicon dioxide, 0.5% sodium polyacrylate and 69.5% water.
[0042] Then it was cleaned with water for a second time. The cleaned micro-reaction channel was placed in a tubular furnace and nitrogen was introduced as a protective gas. The air velocity was controlled at 6h -1 , the temperature was raised to 70°C at a rate of 10°C / min, dried for 12 hours, and then raised to 120°C at a rate of 30°C / min, maintained for 1 hour, and the suspension evenly distributed on the inner wall of the micro-reaction channel was completely solidified. Then the temperature was raised to 200°C at a rate of 30°C / min, and then raised to 350°C at a rate of 20°C / min for 4 hours.
[0043] During the high-temperature calcination process, nickel stearate and copper laurate decompose to form active components - nickel oxide and copper oxide. The gases produced at the same time will form micropores in the cured epoxy resin coating and form an outer surface with a certain roughness (Ra12.5) on the surface. The metal oxides are evenly distributed on the outer surface of the coating and in the micropores. The thickness of the catalyst coating in the microreaction channel is 80μm, thereby preparing a microreaction channel that is resistant to high temperature, high salt and hydrothermal.
[0044] like Figure 1 As shown, the microreactor comprises a steam pipe 1, a storage tank 2, a collecting tank 3, a microreaction channel 5, a reactant input pipe 6 and a distributor 7. The steam pipe 1 is used to pass steam. The storage tank 2 is installed in the steam pipe 1. The collecting tank 3 has a reactant outlet 4, and the collecting tank 3 is installed in the steam pipe 1. The microreaction channel 5 is installed between the storage tank 2 and the collecting tank 3 and is connected thereto. The microreaction channel 5 can be twelve and has a length of seven meters. One end of the reactant input pipe 6 is connected to the storage tank 2, and the other end extends outward through the steam pipe 1. The distributor 7 is installed in the storage tank 2 and is located at the position where the reactant input pipe 6 is connected to the storage tank 2. By passing steam in the steam pipe 1, the reactant enters the distributor 7 and the storage tank 2 through the reactant input pipe 6, and then enters the microreaction channel 5 to react. The product after the reaction is in the collecting tank 3 and discharged through the reactant outlet 4.
[0045] Example 5
[0046] Zinc oleate and cobalt laurate are mixed in a metal atomic molar ratio of 1:1 and then used as a catalyst precursor and mixed with epoxy resin (carbon nanotube epoxy resin) to prepare a glue solution, which is added in a mass ratio of 4% of the catalyst precursor to the carbon nanotube epoxy resin, and the glue solution is slowly injected into a microreactor channel so that the glue solution is evenly distributed on the inner wall of the microreaction channel to form a coating with a porosity of 30%; subsequently, a displacement fluid is used to wash out the remaining catalyst precursor and carbon nanotube epoxy resin, and the displacement fluid is composed of silicon dioxide, polyacrylamide and water, and is configured with a mass fraction of 35% silicon dioxide, 0.7% sodium polyacrylate and 64.3% water.
[0047] Then the microreactor was cleaned with water for a second time. The cleaned microreactor was placed in a tubular furnace and nitrogen was introduced as a protective gas. The air velocity was controlled at 7 h -1 , the temperature was raised to 60°C at a heating rate of 20°C / min, dried for 12 hours, and then raised to 120°C at a heating rate of 20°C / min, maintained for 2 hours, and the suspension evenly distributed on the inner wall of the micro-reaction channel was completely solidified. The temperature was then raised to 200°C at a heating rate of 20°C / min, and then continued to be raised to 450°C at a heating rate of 30°C / min for 2 hours.
[0048] During the high-temperature calcination process, zinc oleate and cobalt laurate decompose to form active components - zinc oxide and cobalt oxide. The gases produced at the same time will form micropores in the cured epoxy resin coating and form an outer surface with a certain roughness on the surface. The metal oxides are evenly distributed on the outer surface of the coating and in the micropores. The thickness of the catalyst coating in the microreaction channel is 90μm, thereby preparing a microreaction channel that is resistant to high temperature, high salt and hydrothermal.
[0049] like Figure 1 As shown, the microreactor comprises a steam pipe 1, a storage tank 2, a collecting tank 3, a microreaction channel 5, a reactant input pipe 6 and a distributor 7. The steam pipe 1 is used to pass steam. The storage tank 2 is installed in the steam pipe 1. The collecting tank 3 has a reactant outlet 4, and the collecting tank 3 is installed in the steam pipe 1. The microreaction channel 5 is installed between the storage tank 2 and the collecting tank 3 and is connected thereto. The microreaction channel 5 can be fifteen and has a length of six meters. One end of the reactant input pipe 6 is connected to the storage tank 2, and the other end extends outward through the steam pipe 1. The distributor 7 is installed in the storage tank 2 and is located at the position where the reactant input pipe 6 is connected to the storage tank 2. By passing steam in the steam pipe 1, the reactant enters the distributor 7 and the storage tank 2 through the reactant input pipe 6, and then enters the microreaction channel 5 to react. The product after the reaction is in the collecting tank 3 and discharged through the reactant outlet 4.
[0050] Example 6
[0051] Cobalt nitrate and zinc nitrate are mixed in a metal atomic molar ratio of 1:2 and then mixed as a catalyst precursor with epoxy resin (carbon nanotube epoxy resin) to prepare a glue solution, which is added in a mass ratio of 5% between the catalyst precursor and the carbon nanotube epoxy resin, and the glue solution is slowly injected into a microreactor channel so that the glue solution is evenly distributed on the inner wall of the microreaction channel to form a coating with a porosity of 20%; subsequently, a displacement fluid is used to wash out the remaining catalyst precursor and carbon nanotube epoxy resin, and the displacement fluid is composed of silicon dioxide, polyacrylamide and water, and is configured with a mass fraction of 40% silicon dioxide, 0.8% polyacrylamide and 59.2% water.
[0052] Then it was cleaned with water for a second time. The cleaned micro-reaction channel was placed in a tubular furnace and nitrogen was introduced as a protective gas. The air velocity was controlled at 9h -1 , the temperature was raised to 80°C at a rate of 30°C / min, dried for 8 hours, and then raised to 120°C at a rate of 15°C / min, maintained for 3 hours, and the suspension evenly distributed on the inner wall of the micro-reaction channel was completely solidified. The temperature was then raised to 200°C at a rate of 25°C / min, and then raised to 400°C at a rate of 30°C / min for 3 hours.
[0053] During the high-temperature calcination process, cobalt nitrate and zinc nitrate decompose to form active components - zinc oxide and cobalt oxide. The gases produced at the same time will form micropores in the cured epoxy resin coating and form an outer surface with a certain roughness on the surface. The metal oxides are evenly distributed on the outer surface of the coating and in the micropores. The thickness of the catalyst coating in the microreaction channel is 75μm, thus preparing a microcatalytic reactor resistant to high temperature, high salt and hydrothermal conditions.
[0054] like Figure 1 As shown, the microreactor comprises a steam pipe 1, a storage tank 2, a collecting tank 3, a micro-reaction channel 5, a reactant input pipe 6 and a distributor 7. The steam pipe 1 is used to pass steam. The storage tank 2 is installed in the steam pipe 1. The collecting tank 3 has a reactant outlet 4, and the collecting tank 3 is installed in the steam pipe 1. The micro-reaction channel 5 is installed between the storage tank 2 and the collecting tank 3 and is connected thereto. The micro-reaction channel 5 can be six and eight meters long. One end of the reactant input pipe 6 is connected to the storage tank 2, and the other end extends outward through the steam pipe 1. The distributor 7 is installed in the storage tank 2 and is located at the position where the reactant input pipe 6 is connected to the storage tank 2. By passing steam in the steam pipe 1, the reactant enters the distributor 7 and the storage tank 2 through the reactant input pipe 6, and then enters the micro-reaction channel 5 to react. The product after the reaction is in the collecting tank 3 and discharged through the reactant outlet 4.
[0055] In the description of this specification, specific features, structures, materials or characteristics may be combined in an appropriate manner in any one or more embodiments or examples.
[0056] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. Micro reaction channel, It is characterized in that The invention comprises a coating attached to the inner wall of a micro-reaction channel, wherein the preparation method of the coating comprises the following steps: A. preparing a catalyst precursor and an epoxy resin into a glue solution, and evenly distributing the glue solution on the inner wall of the micro-reaction channel to form a coating, wherein the epoxy resin includes at least one of epoxy silicone resin, phosphorus-containing epoxy resin, carbon nanotube-reinforced epoxy resin and aluminum-containing epoxy resin; B. preparing a displacement liquid with solid particles, a polymer matrix dispersant and a dispersion medium, and using the displacement liquid to clean the micro-reaction channel to wash out the residual catalyst precursor and epoxy resin, and then washing with water; C. Under a nitrogen protective atmosphere, the micro-reaction channel cleaned in step B is placed in a tube furnace to cure the coating so that the coating forms a microporous structure.
2. The micro-reaction channel according to claim 1, It is characterized in that In step A, the mass ratio of the catalyst precursor to the epoxy resin is 1-5%.
3. The micro-reaction channel according to claim 1, It is characterized in that In step A, the catalyst precursor includes at least one of ferric nitrate nonahydrate, nickel nitrate hexahydrate, iron naphthenate, cobalt stearate, manganese laurate, nickel stearate, copper laurate, zinc oleate, cobalt laurate, cobalt nitrate and zinc nitrate.
4. The micro-reaction channel according to claim 1, It is characterized in that In step A, the coating has a thickness of 1 to 100 μm.
5. The micro-reaction channel according to claim 1, It is characterized in that In step B, based on the total weight percentage of the raw materials, the solid particles are 20-40%, the polymer matrix dispersant is 0.5-1%, and the dispersion medium is 50-98%.
6. The micro-reaction channel according to claim 1, It is characterized in that In step B, the solid particles include at least one of silicon dioxide, corundum and silicon carbide, the particle size of the solid particles is 20 to 500 nm, the polymer matrix dispersant includes at least one of polyacrylamide, polyvinyl alcohol and sodium polyacrylate, and the dispersion medium is water.
7. The micro-reaction channel according to claim 1, It is characterized in that In step C, the coating is cured in the tube furnace to form a microporous structure, which specifically includes the following steps: nitrogen is introduced as a protective gas at an air velocity of 1 to 10 h -1 , heat up to 40-80°C at a heating rate of 5-50°C / min, dry for 6-12h, then heat up to 90-120°C at a heating rate of 5-50°C / min, keep for 1-6h, solidify the coating evenly distributed on the inner wall of the microreaction channel, then continue to heat up to 200°C at a heating rate of 5-10°C / min, and then continue to heat up to 300-450°C at a heating rate of 10-20°C / min, and keep for 2-6h.
8. The micro-reaction channel according to claim 1, It is characterized in that In step C, the porosity of the coating is 10-50%, and the size of the micropores is 10-500 nm.
9. Microreactor, It is characterized in that include: Steam pipe, used to introduce steam; Storage tanks, installed in steam pipes; A collecting tank having a reactant outlet, wherein the collecting tank is installed in the steam pipeline; The micro-reaction channel according to any one of claims 1 to 8, wherein the micro-reaction channel is installed between the storage tank and the collection tank and is in communication therewith; A reactant input pipe, one end of which is connected to the storage tank and the other end of which passes through the steam pipe and extends outward; The distributor is installed in the storage tank and is located at the position where the reactant input pipe is connected to the storage tank.