Preparation method and application of activated carbon composite material
By adding composite coupling agent to activated carbon and generating aluminum/zirconium metal oxides as ternary composite carriers of iron/cobalt elements, the problem of short saturation period of activated carbon in high COD wastewater treatment is solved, and the removal of COD is significantly improved Effect.
Patent Information
- Application Number
- CN202410857213.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-06-28
AI Technical Summary
The existing activated carbon has a short saturation cycle when treating industrial wastewater with high COD content, which limits its application in the field of industrial wastewater treatment.
Add composite coupling agent to activated carbon and generate aluminum/zirconium elements to form metal oxides, which serve as a ternary composite carrier of iron/cobalt elements, provide more active sites, promote the combination of iron/cobalt elements, and improve COD Removal effect.
It significantly improves the removal effect of activated carbon on COD, extends the saturation cycle, and improves the efficiency of wastewater treatment.
Smart Images

Figure CN118491481B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of activated carbon, and relates to a preparation method and application of an activated carbon composite material. Background Art
[0002] Among the many industries that generate wastewater pollution, such as power, chemical, papermaking and other industries, the wastewater discharged during their production process is not only huge in quantity, but also extremely complex in composition. For these wastewaters, the chemical oxygen demand (COD) in them needs to be strictly controlled and removed. Because chemical oxygen demand is a key indicator for measuring the content of organic matter in water bodies, it plays a vital role in water quality detection and water body monitoring. Therefore, these wastewaters must be treated to remove harmful substances.
[0003] Activated carbon adsorption is a common method for treating these industrial wastewaters. It can effectively remove those pollutants that are difficult to treat, thereby improving water quality. However, since the concentration of COD in industrial wastewater is often very high, the saturation cycle of activated carbon is relatively short, which to a certain extent limits the application of activated carbon in the field of industrial wastewater treatment. Therefore, it is necessary to develop an activated carbon that can efficiently remove COD, which is of great significance for solving the problem of industrial wastewater treatment. Summary of the invention
[0004] The purpose of the present invention is to provide a preparation method and application of an activated carbon composite material. The present invention adds a composite coupling agent to the activated carbon, generates aluminum / zirconium elements on its surface to form metal oxides, maintains the original internal structure of the activated carbon, and improves the thermal stability during calcination. Aluminum / zirconium / oxide-activated carbon is a ternary composite carrier of active component iron / cobalt elements, provides more active sites, promotes the binding of more iron / cobalt elements, and significantly improves the removal effect of COD.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for preparing an activated carbon composite material, the preparation method comprising the following steps:
[0007] S1. After placing activated carbon, a mixed auxiliary agent and anhydrous ethanol in a reaction kettle and stirring and dispersing them, a composite coupling agent is added under an inert atmosphere and heated and stirred to obtain a preform;
[0008] S2, adding the nitrate solution and ammonia water into the preform in the reactor in parallel, stirring at a constant temperature, cooling to room temperature, centrifuging and washing the solid to obtain mixed particles;
[0009] S3, after the mixed particles are initially baked, they are placed in a calcining furnace for calcination to obtain an activated carbon composite material.
[0010] As a preferred technical solution of the present invention, in step S1, the stirring and dispersing is stirring at a speed of 600-800 r / min for 45-60 min.
[0011] As a preferred technical solution of the present invention, in step S1, the inert atmosphere is a nitrogen atmosphere; the heating and stirring is stirring at a temperature of 70-75°C for 3-4h.
[0012] As a preferred technical solution of the present invention, in step S1, the mass ratio of the activated carbon, the mixing auxiliary agent, the anhydrous ethanol and the composite coupling agent is 16-18: 0.06-0.09: 50-60: 1.0-1.3.
[0013] As a preferred technical solution of the present invention, in step S1, in step S1, the mixing auxiliary agent is formed by mixing cysteine and EDTA-2Na in a mass ratio of 2:1; the EDTA-2Na is disodium ethylenediaminetetraacetate; the present invention adds a composite coupling agent to the activated carbon, the composite coupling agent fills the internal pores of the activated carbon, decomposes under high-temperature calcination, maintains the original pore structure inside the activated carbon, thereby ensuring the stability of the internal structure of the activated carbon; further, the coordination, hydrogen bonding and electrostatic effects between the mixing auxiliary agent and the composite coupling agent, the mixing auxiliary agent can improve the wettability of the surface of the activated carbon particles while enabling more composite coupling agents to be adsorbed on the internal structure of the activated carbon, and at the same time, the mixing auxiliary agent prevents the occurrence of polycrystalline nucleus agglomeration during the filling process of the iron / cobalt active components.
[0014] As a preferred technical solution of the present invention, in step S1, the composite coupling agent is formed by mixing a zirconate coupling agent and an aluminate coupling agent in a mass ratio of 2:3.5-3.8.
[0015] As a preferred technical solution of the present invention, in step S2, the constant temperature stirring is stirring at a temperature of 70-75°C for 6-8h.
[0016] As a preferred technical solution of the present invention, in step S2, the mass ratio of the nitrate solution, ammonia water and preform is 5.7-6.0:4.0-4.3:50.
[0017] As a preferred technical solution of the present invention, in step S2, the nitrate solution is composed of cobalt nitrate, iron nitrate, sodium nitrate and deionized water in a mass ratio of 2.2:5.0-5.6:0.5-0.8:18-20; further, the addition of sodium nitrate increases the ionic strength of nitrate in the system. Under higher ionic strength, the free movement of iron and cobalt ions is restricted, so that a more uniform precipitation is generated on the activated carbon.
[0018] As a preferred technical solution of the present invention, in step S2, the mass fraction of the ammonia water is 22-25%.
[0019] As a preferred technical solution of the present invention, in step S3, the initial drying is performed at 110-120°C for 1.0-1.5h; the mixed particles contain a large amount of free water, which makes the particles easy to agglomerate and show poor dispersibility, which is not conducive to the smooth progress of the calcination process. In contrast, the dehydrated particles are more fully calcined, thereby facilitating the effective generation of iron / cobalt oxides.
[0020] As a preferred technical solution of the present invention, in step S3, the calcination is performed at a temperature of 480-500° C. for 3-4 hours.
[0021] As a preferred technical solution of the present invention, the aluminate coupling agent is aluminate coupling agent UP-801; and the zirconate coupling agent is zirconate coupling agent DN-807.
[0022] The invention discloses an activated carbon composite material prepared by the above preparation method.
[0023] The invention discloses an application of an activated carbon composite material prepared by the preparation method, and the application of the activated carbon composite material in wastewater treatment.
[0024] Beneficial effects of the present invention:
[0025] The present invention adds a composite coupling agent to the activated carbon, generates aluminum / zirconium elements on its surface to form metal oxides, maintains the original internal structure of the activated carbon, and improves the thermal stability during calcination. Aluminum / zirconium / oxide-activated carbon is a ternary composite carrier of active components of iron / cobalt elements, provides more active sites, promotes the combination of more iron / cobalt elements, and significantly improves the removal effect of COD. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a SEM image before calcination in step S3 of Example 2;
[0027] Figure 2 This is the SEM image after calcination in step S3 in Example 2. DETAILED DESCRIPTION
[0028] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0029] Example 1
[0030] A method for preparing an activated carbon composite material comprises the following steps:
[0031] S1. After placing activated carbon, a mixed auxiliary agent and anhydrous ethanol in a reaction kettle and stirring and dispersing them, a composite coupling agent is added under an inert atmosphere and heated and stirred to obtain a preform;
[0032] In step S1, the stirring and dispersing is stirring at a speed of 600 r / min for 45 minutes; the inert atmosphere is a nitrogen atmosphere; the heating and stirring is stirring at a temperature of 70° C. for 3 hours; the mass ratio of the activated carbon, the mixing auxiliary agent, anhydrous ethanol and the composite coupling agent is 16:0.06:50:1.0; the mixing auxiliary agent is a mixture of cysteine and EDTA-2Na in a mass ratio of 2:1; the composite coupling agent is a mixture of a zirconate coupling agent and an aluminate coupling agent in a mass ratio of 2:3.5;
[0033] S2, adding the nitrate solution and ammonia water into the preform in the reactor in parallel, stirring at a constant temperature, cooling to room temperature, centrifuging and washing the solid to obtain mixed particles;
[0034] In step S2, the constant temperature stirring is stirring at 70°C for 6 hours; the mass ratio of the nitrate solution, ammonia water and preform is 5.7:4.0:50; the nitrate solution is composed of cobalt nitrate, iron nitrate, sodium nitrate and deionized water in a mass ratio of 2.2:5.0:0.5:18; the mass fraction of ammonia water is 22%;
[0035] S3, after pre-baking the mixed particles, placing them in a calcining furnace for calcining to obtain an activated carbon composite material;
[0036] In step S3, the initial baking is performed at 110°C for 1.0 h; and the calcination is performed at 480°C for 3 h.
[0037] Example 2
[0038] A method for preparing an activated carbon composite material comprises the following steps:
[0039] S1. After placing activated carbon, a mixed auxiliary agent and anhydrous ethanol in a reaction kettle and stirring and dispersing them, a composite coupling agent is added under an inert atmosphere and heated and stirred to obtain a preform;
[0040] In step S1, the stirring and dispersing is stirring at a speed of 660 r / min for 50 min; the inert atmosphere is a nitrogen atmosphere; the heating and stirring is stirring at a temperature of 72° C. for 3.3 h; the mass ratio of the activated carbon, the mixing auxiliary agent, anhydrous ethanol and the composite coupling agent is 16.7:0.07:53:1.1; the mixing auxiliary agent is a mixture of cysteine and EDTA-2Na in a mass ratio of 2:1; the composite coupling agent is a mixture of a zirconate coupling agent and an aluminate coupling agent in a mass ratio of 2:3.6;
[0041] S2, adding the nitrate solution and ammonia water into the preform in the reactor in parallel, stirring at a constant temperature, cooling to room temperature, centrifuging and washing the solid to obtain mixed particles;
[0042] In step S2, the constant temperature stirring is stirring at 73°C for 6.5 hours; the mass ratio of the nitrate solution, ammonia water and preform is 5.8:4.1:50; the nitrate solution is composed of cobalt nitrate, iron nitrate, sodium nitrate and deionized water in a mass ratio of 2.2:5.2:0.6:18.7; the mass fraction of ammonia water is 23%;
[0043] S3, after pre-baking the mixed particles, placing them in a calcining furnace for calcining to obtain an activated carbon composite material;
[0044] In step S3, the initial baking is performed at 113°C for 1.2 hours; and the calcination is performed at 480°C for 3.5 hours.
[0045] Example 3
[0046] A method for preparing an activated carbon composite material comprises the following steps:
[0047] S1. After placing activated carbon, a mixed auxiliary agent and anhydrous ethanol in a reaction kettle and stirring and dispersing them, a composite coupling agent is added under an inert atmosphere and heated and stirred to obtain a preform;
[0048] In step S1, the stirring and dispersing is stirring at a speed of 730 r / min for 55 min; the inert atmosphere is a nitrogen atmosphere; the heating and stirring is stirring at a temperature of 74° C. for 3.5 h; the mass ratio of the activated carbon, the mixing auxiliary agent, anhydrous ethanol and the composite coupling agent is 17.3:0.08:57:1.2; the mixing auxiliary agent is a mixture of cysteine and EDTA-2Na in a mass ratio of 2:1; the composite coupling agent is a mixture of a zirconate coupling agent and an aluminate coupling agent in a mass ratio of 2:3.7;
[0049] S2, adding the nitrate solution and ammonia water into the preform in the reactor in parallel, stirring at a constant temperature, cooling to room temperature, centrifuging and washing the solid to obtain mixed particles;
[0050] In step S2, the constant temperature stirring is stirring at 74°C for 7.5 hours; the mass ratio of the nitrate solution, ammonia water and preform is 5.9:4.2:50; the nitrate solution is composed of cobalt nitrate, iron nitrate, sodium nitrate and deionized water in a mass ratio of 2.2:5.4:0.7:19.3; the mass fraction of ammonia water is 24%;
[0051] S3, after pre-baking the mixed particles, placing them in a calcining furnace for calcining to obtain an activated carbon composite material;
[0052] In step S3, the initial baking is performed at 115°C for 1.5 hours; and the calcination is performed at 490°C for 3.5 hours.
[0053] Example 4
[0054] A method for preparing an activated carbon composite material comprises the following steps:
[0055] S1. After placing activated carbon, a mixed auxiliary agent and anhydrous ethanol in a reaction kettle and stirring and dispersing them, a composite coupling agent is added under an inert atmosphere and heated and stirred to obtain a preform;
[0056] In step S1, the stirring and dispersing is stirring at a speed of 800 r / min for 60 min; the inert atmosphere is a nitrogen atmosphere; the heating and stirring is stirring at a temperature of 75° C. for 4 h; the mass ratio of the activated carbon, the mixing auxiliary agent, anhydrous ethanol and the composite coupling agent is 18:0.09:60:1.3; the mixing auxiliary agent is a mixture of cysteine and EDTA-2Na in a mass ratio of 2:1; the composite coupling agent is a mixture of a zirconate coupling agent and an aluminate coupling agent in a mass ratio of 2:3.8;
[0057] S2, adding the nitrate solution and ammonia water into the preform in the reactor in parallel, stirring at a constant temperature, cooling to room temperature, centrifuging and washing the solid to obtain mixed particles;
[0058] In step S2, the constant temperature stirring is stirring at 75°C for 8 hours; the mass ratio of the nitrate solution, ammonia water and preform is 6.0:4.3:50; the nitrate solution is composed of cobalt nitrate, iron nitrate, sodium nitrate and deionized water in a mass ratio of 2.2:5.6:0.8:20; the mass fraction of ammonia water is 25%;
[0059] S3, after pre-baking the mixed particles, placing them in a calcining furnace for calcining to obtain an activated carbon composite material;
[0060] In step S3, the initial baking is performed at 120°C for 1.5 hours; and the calcination is performed at 500°C for 4 hours.
[0061] Comparative Example 1
[0062] Compared with Example 2, the difference is that the mixing auxiliary agent in Comparative Example 1 is cysteine, and the rest remains unchanged.
[0063] Comparative Example 2
[0064] Compared with Example 2, the difference is that the mixing auxiliary agent in Comparative Example 2 is EDTA-2Na, and the rest remains unchanged.
[0065] Comparative Example 3
[0066] Compared with Example 2, the difference is that no mixing auxiliary agent is used in Comparative Example 3, and the rest remains unchanged.
[0067] Comparative Example 4
[0068] Compared with Example 2, the difference is that the composite coupling agent of Comparative Example 4 is a zirconate coupling agent, and the rest remains unchanged.
[0069] Comparative Example 5
[0070] Compared with Example 2, the difference is that the composite coupling agent of Comparative Example 5 is an aluminate coupling agent, and the rest remains unchanged.
[0071] Comparative Example 6
[0072] Compared with Example 2, the difference is that no composite coupling agent is used in Comparative Example 6, and the rest remains unchanged.
[0073] Comparative Example 7
[0074] Compared with Example 2, the difference is that comparative example 7 does not use sodium nitrate, and the rest remains unchanged.
[0075] Comparative Example 8
[0076] Compared with Example 2, the difference is that Comparative Example 8 does not undergo initial baking, and the rest remain unchanged.
[0077] The activated carbons prepared in Examples 1-4 and Comparative Examples 1-8 were tested as follows, and the test results are shown in Table 1.
[0078] Industrial wastewater with a COD of 600 mg / L was used. COD removal rate: According to standard GB 11914-89, the COD removal rate of the activated carbon prepared in Examples 1-4 and Comparative Examples 1-8 was measured;
[0079] COD removal rate (%) = (COD0-COD1) / COD0×100%;
[0080] Where: COD0 is the COD value of wastewater before treatment;
[0081] COD1 is the COD value of the treated wastewater.
[0082] The results are shown in Table 1.
[0083] Table 1
[0084]
[0085] It can be seen from the test results in Table 1 that compared with Comparative Examples 1-8, the activated carbon prepared by Examples 1-4 of the present invention has excellent COD removal performance. This is because the present invention introduces a composite coupling agent into the activated carbon to effectively fill its internal hollow part during the calcination process, thereby significantly suppressing the structural collapse phenomenon caused by stress when the activated carbon is used as a wastewater treatment material. At the same time, with the addition of a mixing auxiliary agent, during the filling process of the composite coupling agent, the mixing auxiliary agent can be adsorbed on the surface of the activated carbon particles, thereby improving the wettability of the surface of the activated carbon particles and effectively preventing the occurrence of polycrystalline nucleus agglomeration. During the calcination process, the mixing auxiliary agent is carbonized, thereby achieving carbon coating on the surface of the activated carbon particles; and the carbonization of the composite coupling agent achieves internal carbon coating. In addition, aluminum / zirconium elements form metal oxides during the calcination process, which not only improves the thermal stability of the activated carbon calcination process and ensures the stability of the activated carbon structure, but also enables the activated carbon to maintain a large number of pore structures. Aluminum / zirconium oxides can also be used as carriers of active components. When aluminum / zirconium elements are compounded to form composite particles, they can reduce their own agglomeration, thereby improving the dispersion of metals, forming smaller metal oxide particles, and more evenly distributed on the activated carbon, thereby providing more active sites. This allows more active components to be loaded on the aluminum-zirconium-activated carbon ternary composite carrier. In addition, the interconnected pore structure on the ternary composite carrier also promotes the rapid combination of active elements iron and cobalt with active sites, thereby significantly improving the removal effect of COD.
[0086] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for preparing an activated carbon composite material, characterized in that: The preparation method comprises the following steps: S1. After placing activated carbon, a mixing aid and anhydrous ethanol in a reaction kettle and stirring and dispersing them, a composite coupling agent is added under an inert atmosphere and heated and stirred to obtain a preform; the mixing aid is prepared by mixing cysteine and EDTA-2Na in a mass ratio of 2:1; the composite coupling agent is prepared by mixing a zirconate coupling agent and an aluminate coupling agent in a mass ratio of 2:3.5-3.8; the mass ratio of the activated carbon, the mixing aid, the anhydrous ethanol and the composite coupling agent is 16-18:0.06-0.09:50-60:1.0-1.3; S2, adding nitrate solution and ammonia water to the preform of the reactor in parallel, stirring at a constant temperature, cooling to room temperature, centrifuging and washing the solid to obtain mixed particles; the mass ratio of cobalt nitrate, iron nitrate, sodium nitrate and deionized water in the nitrate solution is 2.2:5.0-5.6:0.5-0.8:18-20; the mass fraction of ammonia water is 22-25%; S3, after the mixed particles are initially baked, they are placed in a calcining furnace for calcination to obtain an activated carbon composite material.
2. The method for preparing an activated carbon composite material according to claim 1, characterized in that: In step S1, the stirring and dispersing is stirring at a speed of 600-800 r / min for 45-60 min; the inert atmosphere is a nitrogen atmosphere; and the heating and stirring is stirring at a temperature of 70-75° C. for 3-4 h.
3. The method for preparing an activated carbon composite material according to claim 1, characterized in that: In step S2, the constant temperature stirring is stirring at 70-75°C for 6-8h.
4. The method for preparing an activated carbon composite material according to claim 1, characterized in that: In step S2, the mass ratio of the nitrate solution, the ammonia water and the preform is 5.7-6.0:4.0-4.3:
50.
5. The method for preparing an activated carbon composite material according to claim 1, characterized in that: In step S3, the initial baking is drying at 110-120°C for 1.0-1.5h; and the calcination is calcining at 480-500°C for 3-4h.
6. An activated carbon composite material prepared by the preparation method according to any one of claims 1 to 5.
7. An application of an activated carbon composite material prepared by the preparation method according to any one of claims 1 to 5, characterized in that: Application of the activated carbon composite material in wastewater treatment.
Citation Information
Patent Citations
Activated carbon composite material for capacitor electrode and preparation method thereof
CN116013703A
Environment-friendly regenerated activated carbon and preparation method thereof
CN117563562A