A process for separating harmful components from degradable packaging waste and then reusing them
Through the NaOH solution selective dissolution and flotation technology, combined with near-critical water decomposition and surfactant modification, the problem of metal and plastic mixed in packaging waste is solved, and the separation of harmful components is achieved and the efficiency of epoxy resin composite materials is achieved. Preparation improves the mechanical properties and reuse value of the material.
Patent Information
- Application Number
- CN202410923894.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-11
AI Technical Summary
The prior art is difficult to effectively deal with packaging waste containing metals and plastics, resulting in the inability to effectively separate and reuse harmful components, and the existing degradable packaging materials naturally degrade slowly.
The NaOH solution is used to selectively dissolve and sort metal components, combine flotation technology of sodium lignin sulfonate and pineol oil, followed by near-critical water decomposition and surfactant modification, and finally prepare epoxy resin composites.
It realizes effective separation and reuse of harmful components in packaging waste, improves the decomposition speed of resin materials, the generation speed and uniformity of epoxy resin composite materials, and improves the mechanical properties of the material.
Smart Images

Figure CN118492037B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waste recycling and reuse, and in particular to a process for separating harmful components of degradable packaging waste and then reusing them. Background Art
[0002] With the vigorous development of the packaging industry and the improvement of people's living standards, packaging consumption is increasing day by day. It is widely used in machinery, automobiles, home appliances, light industry, electronics, food processing and other industries.
[0003] Compared with the continuous growth in application, the recycling of packaging and turnover waste is not optimistic. The existing packaging waste is mainly plastic, that is, thermosetting resin material, and a small amount of metal material is used for pharmaceutical packaging. These packaging wastes are directly discarded by people after losing their use value. Although most of the current packaging materials are degradable materials, the degradation rate in nature is slow, and some packaging wastes have the possibility and value of secondary utilization. However, due to the mixed components in the packaging waste, metal packaging and plastic packaging cannot be treated together. Treating packaging waste containing metal packaging in the same way as plastic packaging will result in the presence of harmful components in the waste. Therefore, a process is needed to separate the harmful components of degradable packaging waste and then perform secondary processing and utilization to solve the problems existing in the prior art. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a process for separating harmful components of degradable packaging waste and then reusing them.
[0005] A process for separating harmful components from degradable packaging waste and then reusing them comprises the following steps:
[0006] S1: Selective dissolution and separation of metal components in degradable packaging waste
[0007] The degradable packaging waste is immersed in a NaOH solution and heated to leach the metal in the waste, and then the filtrate is removed by filtering, and the filter residue is dried to obtain the treated waste, and sodium lignin sulfonate is selected as a wetting agent and mixed with pine oil to obtain a mixed solution, and the treated waste is immersed in the mixed solution for flotation, and the sedimentation part is collected and air-dried to obtain a flotation material;
[0008] S2: Mixed molding of flotation material and additives
[0009] The flotation material is crushed and vibrated and screened, and then fully mixed with the additive to form a mixed powder, and the mixed powder is sent to a hot press for molding to obtain a new material;
[0010] S3: New materials for near-critical water decomposition
[0011] Put the new material into a reactor, add distilled water, and then add a catalyst phenol, seal the reactor and put it into a salt bath furnace at 300-305°C, continue the reaction, take out the reactor after the reaction is finished, put it into cold water to quench it, collect the water phase decomposition product with a collection bottle, add ethyl acetate to the water phase decomposition product for extraction, separate the extract to obtain a solid phase product, soak the solid phase product in ethyl acetate, and then soak it in distilled water, take it out and dry it to obtain a decomposition product;
[0012] S4: Surface treatment of decomposition products
[0013] The decomposition product is mechanically crushed and then sieved to obtain a decomposition product powder, the decomposition product powder is added to a reaction bottle containing an ethanol solution until it is completely immersed, KH550 is added, stirred for reaction, to obtain a treatment liquid, and the treatment liquid is dried to obtain a modified powder;
[0014] S5: Preparation of epoxy resin composites using modified powders
[0015] Add the modified powder into a beaker containing epoxy resin, then add a defoaming agent, mechanically stir and ultrasonically disperse, to obtain intermediate I, add curing agent DDM to intermediate I, stir evenly and degas in vacuum, finally cast into a polytetrafluoroethylene mold, heat and cure in a blast drying oven to obtain intermediate II, place intermediate II in a blast drying oven and slowly cool to room temperature to obtain intermediate III, take out intermediate III from the blast drying oven, and place it for 24-26 hours to obtain an epoxy resin composite material.
[0016] Furthermore, step S1 selectively dissolving and sorting the metal components of the degradable packaging waste includes the following steps:
[0017] S1.1: Immerse the degradable packaging waste in NaOH solution for 15-20 minutes, liquid-to-solid ratio (15-20): 1, NaOH concentration 1-1.25 mol / L, raise the temperature to 60-70°C, leach the metals in the waste, then filter out the filtrate, dry the residue, and obtain the treated waste;
[0018] S1.2: 6000 mg / L sodium lignin sulfonate is selected as a wetting agent, mixed with 5 mg / L pine oil to obtain a mixed solution, the treated waste is immersed in the mixed solution, and flotation is performed under the conditions of adjusting the flotation time to 15-20 min and the flotation time to 15-20 min. The sedimentation part is collected and air-dried at 60°C for 6-7 hours to obtain a flotation material.
[0019] Furthermore, step S2 of mixing the flotation material with the additive material for molding comprises the following steps:
[0020] S2.1: The flotation material is crushed and vibrated for 15-20 minutes, and then fully mixed with the additive for 15-20 minutes. The mass ratio of the flotation material to the additive is (2-4):1 to form a mixed powder;
[0021] S2.2: The mixed powder is sent to a hot press for compression molding. The compression pressure of the hot press is 10-12 MPa, the compression temperature is 150-160°C, and the compression time is 5-7 minutes during heating to obtain a new material.
[0022] Further, step S3 near-critical water decomposition of new materials comprises the following steps:
[0023] S3.1: Weigh and record the mass of the new material, then put the weighed new material into the reactor, add distilled water according to the material-liquid mass ratio of 1:(8-10), then add 0.2-0.5% of the total volume of catalyst phenol with a concentration of 0.4-0.7 mol / L, and seal the reactor;
[0024] S3.2: Place the reactor in a salt bath furnace heated to a specified temperature of 300-305°C and continue the reaction for 45-60 minutes;
[0025] S3.3: After completion, remove the reactor and place it in cold water to quench it. After leaving it for 15-20 minutes, open the reactor and collect the aqueous phase decomposition product in a collection bottle. Add ethyl acetate to the aqueous phase decomposition product for extraction. After 100-120 minutes, separate the extract to obtain a solid phase product.
[0026] S3.4: Place the solid phase product in ethyl acetate, soak for 20-24 hours, and then soak in distilled water for 2-3 hours. After taking it out, dry it in an oven at a temperature of 100-110°C to obtain a decomposition product.
[0027] Furthermore, step S4, surface treatment of the decomposition product, comprises the following steps:
[0028] S4.1: The decomposition product is mechanically crushed and passed through a 200-mesh sieve to obtain a decomposition product powder, the decomposition product powder is added to a reaction bottle filled with an ethanol solution with a volume fraction of 80-95% until it is completely immersed, 1-3% of the mass of the decomposition product powder is added with KH550, and the mixture is stirred and reacted in an intelligent oil bath pot at 65-80°C for 10-12h to obtain a treated liquid;
[0029] S4.2: Dry the treated liquid in a forced air drying oven at 100° C. to obtain a modified powder.
[0030] Furthermore, step S5 of modifying the powder to prepare the epoxy resin composite material comprises the following steps:
[0031] S5.1: Add the modified powder into a beaker containing epoxy resin, add a defoamer, stir mechanically at 65-80°C for 20-30 min, and then continue to ultrasonically disperse at 65-80°C for 50-60 min to obtain intermediate I;
[0032] S5.2: Add 25-28% of the mass of intermediate I to curing agent DDM into intermediate I, stir evenly and transfer to a vacuum drying oven at 60-80°C for vacuum degassing for 8-10 minutes, and finally cast into a polytetrafluoroethylene mold preheated at 60-80°C, heat and cure in a blast drying oven, the curing conditions are 100°C for 1 hour, then 136°C for 2 hours, and finally 160°C for 1 hour, to obtain intermediate II;
[0033] S5.3: Place intermediate II in a forced air drying oven and slowly cool to room temperature to obtain intermediate III;
[0034] S5.4: Take out intermediate III from the forced air drying oven and leave it for 24-26 hours to obtain an epoxy resin composite material.
[0035] Furthermore, in step S1, the volume ratio of sodium lignin sulfonate to pine oil is 1:(0.5-1.5).
[0036] Furthermore, the additive in step S2 is one or more of thermosetting phenolic plastics, thermoplastic high-density polyethylene, polypropylene and polyvinyl chloride.
[0037] Furthermore, in step S5.1, the volume ratio of the modified powder, epoxy resin and defoaming agent is 1:(8-10):(1-2).
[0038] Furthermore, the defoaming agent in step S5.1 is specifically a silicone defoaming agent.
[0039] Compared with the prior art, the present invention has at least the following beneficial effects:
[0040] 1. The present invention places the molded packaging waste into a salt bath furnace and heats it to above 300° C. for near-critical hydrolysis, and adds a catalyst phenol to destroy the resin structure in the packaging waste. The main components in the packaging waste, namely various resin materials, are decomposed by near-critical hydrolysis, and the catalyst phenol further promotes the breaking of chemical bonds of the resin material, thereby accelerating the decomposition speed and decomposing the resin into small molecular materials, which are convenient for subsequent reuse.
[0041] 2. The present invention selectively dissolves and sorts the packaging waste by immersing it in NaOH, thereby dissolving the aluminum-based packaging materials in the packaging waste, such as pharmaceutical aluminum foil, and removes them by filtering and sorting, thereby screening out most of the harmful metal components in the packaging waste, so that the main component of the packaging waste is mainly resin material, thereby subsequently decomposing and recycling the resin material.
[0042] 3. The present invention utilizes KH550 surfactant to modify the surface of the decomposition product, thereby preventing the decomposition product powder from agglomerating during the subsequent preparation of the epoxy resin composite material, and increasing the contact area between the epoxy resin and the modified powder, thereby increasing the generation speed and internal uniformity of the epoxy resin composite material and improving the quality of the epoxy resin composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] The accompanying drawings, which are incorporated herein and constitute a part of the specification, illustrate embodiments of the present disclosure and, together with the description, further serve to explain the principles of the present disclosure and to enable those skilled in the relevant art to make and use the present disclosure.
[0044] Figure 1 This is a process flow chart for separating and reusing harmful components of degradable packaging waste adopted in an embodiment of the present invention. DETAILED DESCRIPTION
[0045] The following is a detailed description of a process for separating harmful components from degradable packaging waste and then reusing it in combination with the accompanying drawings and specific embodiments. At the same time, it is explained here that in order to make the embodiments more detailed, the following embodiments are the best and preferred embodiments, and those skilled in the art may also adopt other alternatives to implement some known technologies; and the accompanying drawings are only for more specific description of the embodiments, and are not intended to specifically limit the present invention.
[0046] Embodiment 1:
[0047] A process for separating harmful components from degradable packaging waste and then reusing them, such as Figure 1 As shown, the following steps are included:
[0048] S1: Selective dissolution and separation of metal components in degradable packaging waste
[0049] S1.1: Immerse the degradable packaging waste in NaOH solution for 20 minutes, with a liquid-to-solid ratio of 20:1 and a NaOH concentration of 1.25 mol / L. Raise the temperature to 70°C to leach the metals in the waste. Then filter out the filtrate, dry the residue, and obtain the treated waste.
[0050] S1.2: 6000 mg / L sodium lignin sulfonate was selected as a wetting agent and mixed with 5 mg / L pine oil. The volume ratio of sodium lignin sulfonate to pine oil was 1:1.5 to obtain a mixed solution. The treated waste was immersed in the mixed solution and flotation was performed under the conditions of adjustment time of 20 min and flotation time of 20 min. The sedimentation part was collected and air-dried at 60°C for 7 h to obtain a flotation material.
[0051] S2: Mixed molding of flotation material and additives
[0052] S2.1: The flotation material is crushed and vibrated for 15 minutes, and then fully mixed with the additive for 20 minutes. The additive is a thermosetting phenolic plastic. The mass ratio of the flotation material to the additive is 2:1 to form a mixed powder.
[0053] S2.2: The mixed powder is sent into a hot press for compression molding, the compression pressure of the hot press is 12 MPa, the compression temperature is 160°C, and the compression time is 7 min during heating to obtain a new material;
[0054] S3: New materials for near-critical water decomposition
[0055] S3.1: Weigh and record the mass of the new material, then put the weighed new material into the reactor, add distilled water according to the material-liquid ratio of 1:10, and then add 0.5% of the total volume of catalyst phenol with a concentration of 0.7 mol / L, and seal the reactor;
[0056] S3.2: Place the reactor in a salt bath furnace heated to a specified temperature of 305°C and continue the reaction for 60 minutes;
[0057] S3.3: After the reaction is completed, the reactor is taken out and placed in cold water for rapid cooling. After 20 minutes, the reactor is opened and the aqueous phase decomposition product is collected in a collection bottle. Ethyl acetate is added to the aqueous phase decomposition product for extraction. After 120 minutes, the extract is separated to obtain a solid phase product.
[0058] S3.4: The solid phase product is placed in ethyl acetate and soaked for 24 hours, and then soaked in distilled water for 2 hours. After being taken out, it is dried in an oven at a temperature of 110°C to obtain a decomposition product;
[0059] S4: Surface treatment of decomposition products
[0060] S4.1: The decomposition product is mechanically crushed and passed through a 200-mesh sieve to obtain a decomposition product powder, the decomposition product powder is added to a reaction bottle filled with a 95% ethanol solution by volume until it is completely immersed, 3% of the mass of the decomposition product powder is added with KH550, and the mixture is stirred and reacted in an intelligent oil bath at 80°C for 12 hours to obtain a treated solution;
[0061] S4.2: Dry the treated liquid in a forced air drying oven at 100° C. to obtain a modified powder.
[0062] S5: Preparation of epoxy resin composites using modified powders
[0063] S5.1: Add the modified powder to a beaker containing epoxy resin, and then add a silicone defoamer, the volume ratio of the modified powder, epoxy resin and defoamer is 1:10:2, and then mechanically stir at 80°C for 30 minutes and then continue to ultrasonically disperse at 80°C for 60 minutes to obtain intermediate I;
[0064] S5.2: Add 28% of the mass of intermediate I in the curing agent DDM to intermediate I, stir evenly and transfer to a vacuum drying oven at 80°C for vacuum degassing for 10 min, and finally cast into a polytetrafluoroethylene mold preheated at 80°C, heat and cure in a blast drying oven. The curing conditions are 100°C for 1 h, then 136°C for 2 h, and finally 160°C for 1 h, to obtain intermediate II;
[0065] S5.3: Place intermediate II in a forced air drying oven and slowly cool to room temperature to obtain intermediate III;
[0066] S5.4: Take out intermediate III from the forced air drying oven and leave it for 26 hours to obtain an epoxy resin composite material.
[0067] Embodiment 2:
[0068] A process for separating harmful components from degradable packaging waste and then reusing them, such as Figure 1 As shown, the following steps are included:
[0069] S1: Selective dissolution and separation of metal components in degradable packaging waste
[0070] S1.1: Immerse the degradable packaging waste in NaOH solution for 20 minutes, with a liquid-to-solid ratio of 15:1 and a NaOH concentration of 1.25 mol / L. Raise the temperature to 70°C to leach the metals in the waste. Then filter out the filtrate, dry the residue, and obtain the treated waste.
[0071] S1.2: 6000 mg / L sodium lignin sulfonate was selected as a wetting agent and mixed with 5 mg / L pine oil. The volume ratio of sodium lignin sulfonate to pine oil was 1:1 to obtain a mixed solution. The treated waste was immersed in the mixed solution and flotation was performed under the conditions of adjusting the flotation time for 20 min and the flotation time for 20 min. The sedimentation part was collected and air-dried at 60°C for 7 h to obtain a flotation material.
[0072] S2: Mixed molding of flotation material and additives
[0073] S2.1: The flotation material is crushed and vibrated for 15 minutes, and then fully mixed with the additive for 20 minutes. The additive is a thermosetting phenolic plastic. The mass ratio of the flotation material to the additive is 4:1 to form a mixed powder.
[0074] S2.2: The mixed powder is sent into a hot press for compression molding, the compression pressure of the hot press is 12 MPa, the compression temperature is 160°C, and the compression time is 7 min during heating to obtain a new material;
[0075] S3: New materials for near-critical water decomposition
[0076] S3.1: Weigh and record the mass of the new material, then put the weighed new material into the reactor, add distilled water according to the material-liquid ratio of 1:8, and then add 0.5% of the total volume of catalyst phenol with a concentration of 0.7 mol / L, and seal the reactor;
[0077] S3.2: Place the reactor in a salt bath furnace heated to a specified temperature of 305°C and continue the reaction for 60 minutes;
[0078] S3.3: After the reaction is completed, the reactor is taken out and placed in cold water for rapid cooling. After 20 minutes, the reactor is opened and the aqueous phase decomposition product is collected in a collection bottle. Ethyl acetate is added to the aqueous phase decomposition product for extraction. After 120 minutes, the extract is separated to obtain a solid phase product.
[0079] S3.4: The solid phase product is placed in ethyl acetate and soaked for 24 hours, and then soaked in distilled water for 2 hours. After being taken out, it is dried in an oven at a temperature of 110°C to obtain a decomposition product;
[0080] S4: Surface treatment of decomposition products
[0081] S4.1: The decomposition product is mechanically crushed and passed through a 200-mesh sieve to obtain a decomposition product powder, the decomposition product powder is added to a reaction bottle filled with a 95% by volume ethanol solution until it is completely immersed, 1% by weight of the decomposition product powder is added with KH550, and the mixture is stirred and reacted in an intelligent oil bath at 80°C for 12 hours to obtain a treatment solution;
[0082] S4.2: Dry the treated liquid in a forced air drying oven at 100° C. to obtain a modified powder.
[0083] S5: Preparation of epoxy resin composites using modified powders
[0084] S5.1: Add the modified powder to a beaker containing epoxy resin, and then add a silicone defoamer, the volume ratio of the modified powder, epoxy resin and defoamer is 1:8:1, and then mechanically stir at 80°C for 30 minutes and then continue to ultrasonically disperse at 80°C for 60 minutes to obtain intermediate I;
[0085] S5.2: Add 28% of the mass of intermediate I in the curing agent DDM to intermediate I, stir evenly and transfer to a vacuum drying oven at 80°C for vacuum degassing for 10 min, and finally cast into a polytetrafluoroethylene mold preheated at 80°C, heat and cure in a blast drying oven. The curing conditions are 100°C for 1 h, then 136°C for 2 h, and finally 160°C for 1 h, to obtain intermediate II;
[0086] S5.3: Place intermediate II in a forced air drying oven and slowly cool to room temperature to obtain intermediate III;
[0087] S5.4: Take out intermediate III from the forced air drying oven and leave it for 26 hours to obtain an epoxy resin composite material.
[0088] Embodiment 3:
[0089] A process for separating harmful components from degradable packaging waste and then reusing them, such as Figure 1 As shown, the following steps are included:
[0090] S1: Selective dissolution and separation of metal components in degradable packaging waste
[0091] S1.1: Immerse the degradable packaging waste in NaOH solution for 15 min, with a liquid-to-solid ratio of 20:1 and a NaOH concentration of 1.25 mol / L. Raise the temperature to 60°C to leach the metals in the waste. Then filter out the filtrate, dry the residue, and obtain the treated waste.
[0092] S1.2: 6000 mg / L sodium lignin sulfonate was selected as a wetting agent and mixed with 5 mg / L pine oil. The volume ratio of sodium lignin sulfonate to pine oil was 1:1.5 to obtain a mixed solution. The treated waste was immersed in the mixed solution and flotation was performed under the conditions of adjusting the flotation time to 15 min and the flotation time to 15 min. The sedimentation part was collected and air-dried at 60°C for 6 h to obtain a flotation material.
[0093] S2: Mixed molding of flotation material and additives
[0094] S2.1: The flotation material is crushed and vibrated for 20 minutes, and then fully mixed with the additive for 15 minutes. The additive is a thermosetting phenolic plastic. The mass ratio of the flotation material to the additive is 2:1 to form a mixed powder.
[0095] S2.2: The mixed powder is sent into a hot press for compression molding, the compression pressure of the hot press is 10 MPa, the compression temperature is 150°C, and the compression time is 5 min during heating to obtain a new material;
[0096] S3: New materials for near-critical water decomposition
[0097] S3.1: Weigh and record the mass of the new material, then put the weighed new material into the reactor, add distilled water according to the material-liquid ratio of 1:10, and then add 0.5% of the total volume of catalyst phenol with a concentration of 0.7 mol / L, and seal the reactor;
[0098] S3.2: Place the reactor in a salt bath furnace heated to a specified temperature of 300°C and continue the reaction for 50 minutes;
[0099] S3.3: After completion, remove the reactor and place it in cold water to quench it. After 20 minutes, open the reactor and collect the aqueous phase decomposition product in a collection bottle. Add ethyl acetate to the aqueous phase decomposition product for extraction. After 100 minutes, separate the extract to obtain a solid phase product.
[0100] S3.4: The solid phase product is placed in ethyl acetate and soaked for 20 hours, and then soaked in distilled water for 3 hours. After being taken out, it is dried in an oven at a temperature of 110°C to obtain a decomposition product;
[0101] S4: Surface treatment of decomposition products
[0102] S4.1: The decomposition product is mechanically crushed and passed through a 200-mesh sieve to obtain a decomposition product powder, the decomposition product powder is added to a reaction bottle containing a 95% by volume ethanol solution until it is completely immersed, 3% by mass of the decomposition product powder is added with KH550, and the mixture is stirred and reacted in an intelligent oil bath at 70°C for 10 hours to obtain a treated solution;
[0103] S4.2: Dry the treated liquid in a forced air drying oven at 100° C. to obtain a modified powder.
[0104] S5: Preparation of epoxy resin composites using modified powders
[0105] S5.1: Add the modified powder to a beaker containing epoxy resin, and then add a silicone defoamer, the volume ratio of the modified powder, epoxy resin and defoamer is 1:10:2, and then mechanically stir at 70°C for 30 minutes and then continue to ultrasonically disperse at 70°C for 50 minutes to obtain intermediate I;
[0106] S5.2: Add 28% of the mass of intermediate I in the curing agent DDM to intermediate I, stir evenly and transfer to a vacuum drying oven at 80°C for vacuum degassing for 10 min, and finally cast into a polytetrafluoroethylene mold preheated at 80°C, heat and cure in a blast drying oven. The curing conditions are 100°C for 1 h, then 136°C for 2 h, and finally 160°C for 1 h, to obtain intermediate II;
[0107] S5.3: Place intermediate II in a forced air drying oven and slowly cool to room temperature to obtain intermediate III;
[0108] S5.4: Take out intermediate III from the forced air drying oven and leave it for 26 hours to obtain an epoxy resin composite material.
[0109] Comparative Example 1:
[0110] Compared with Example 1, the difference of Comparative Example 1 is that the catalyst phenol is not added in step S3, specifically: "S3.1: weigh and record the mass of the new material, then put the weighed new material into the reactor, and add distilled water according to a material-liquid ratio of 1:10, and seal the reactor;
[0111] S3.2: Place the reactor in a salt bath furnace heated to a specified temperature of 305°C and continue the reaction for 60 minutes;
[0112] S3.3: After the reaction is completed, the reactor is taken out and placed in cold water for rapid cooling. After 20 minutes, the reactor is opened and the aqueous phase decomposition product is collected in a collection bottle. Ethyl acetate is added to the aqueous phase decomposition product for extraction. After 120 minutes, the extract is separated to obtain a solid phase product.
[0113] S3.4: The solid phase product is placed in ethyl acetate and soaked for 24 hours, and then soaked in distilled water for 2 hours. After being taken out, it is dried in an oven at a temperature of 110° C. to obtain a decomposition product. The prepared epoxy resin composite material is recorded as Comparative Example 1.
[0114] Comparative Example 2:
[0115] Compared with Example 1, the difference of Comparative Example 2 is that step S1 is not performed, and the degradable packaging waste is directly used instead of the flotation material to perform step S2, specifically: "S2.1: crushing the flotation material and vibrating and screening it for 15 minutes, and then fully mixing it with the additive for 15-20 minutes, the additive is a thermosetting phenolic plastic, and the mass ratio of the flotation material to the additive is 2:1, to form a mixed powder;
[0116] S2.2: The mixed powder is sent into a hot press for compression molding. The compression pressure of the hot press is 12 MPa, the compression temperature is 160°C, and the compression time is 7 min during heating to obtain a new material. The prepared epoxy resin composite material is recorded as Comparative Example 2.
[0117] Comparative Example 3
[0118] Compared with Example 1, the difference of Comparative Example 3 is that step S4 is not performed, the decomposition product obtained in step S3 is directly crushed through a 200-mesh sieve to obtain a decomposition product powder, and the modified powder in step S5 is replaced by the decomposition product powder, specifically: "S5.1: adding the decomposition product powder to a beaker containing epoxy resin, and then adding an organosilicon defoamer, the volume ratio of the decomposition product powder, the epoxy resin and the defoamer is 1:10:2, and mechanically stirring at 80°C for 30 minutes and then ultrasonically dispersing at 80°C for 60 minutes to obtain intermediate I;
[0119] S5.2: Add 28% of the mass of intermediate I in the curing agent DDM to intermediate I, stir evenly and transfer to a vacuum drying oven at 80°C for vacuum degassing for 10 min, and finally cast into a polytetrafluoroethylene mold preheated at 80°C, heat and cure in a blast drying oven. The curing conditions are 100°C for 1 h, then 136°C for 2 h, and finally 160°C for 1 h, to obtain intermediate II;
[0120] S5.3: Place intermediate II in a forced air drying oven and slowly cool to room temperature to obtain intermediate III;
[0121] S5.4: Take out intermediate III from the blast drying oven and leave it for 26 hours to obtain an epoxy resin composite material, which is recorded as Comparative Example 3.
[0122] Mechanical properties test
[0123] The tensile properties were tested on a UT-2080 electronic tensile testing machine produced by Taiwan Uni-Tech Co., Ltd. according to GB / T528-2009. The embodiments and comparative examples were tested 5 times, and the results were averaged, as shown in Table 1.
[0124] Table 1. Tensile strength and elongation at break
[0125]
[0126] It can be seen that the tensile strengths of Examples 1-3 are 5.72 MPa, 5.66 MPa and 5.68 MPa, respectively, and the elongations at break are 419%, 422% and 417%, respectively, while the tensile strength of Comparative Example 1 is only 2.35 MPa, and the elongation at break is 402%. This is because without the participation of the catalyst phenol, the decomposition strength and rate of the packaging waste are insufficient, resulting in incomplete decomposition of the decomposition products, uneven internal distribution of the obtained epoxy resin composite material, and low tensile strength;
[0127] The tensile strength of Comparative Example 2 is 5.27 MPa, and the elongation at break is 415%. This is because, although the metal material mixed in the packaging waste is not completely removed, a part of it is removed by flotation, and it is crushed into powder and molded and then uniformly mixed with the resin material in the packaging waste. Therefore, it has little effect on the tensile strength of the epoxy resin composite material, which is only slightly inferior to Examples 1-3.
[0128] In Comparative Example 3, the tensile strength is 4.16 MPa and the elongation at break is 378%. It can be seen that the decomposition product powder without KH550 modification is easier to agglomerate, so the internal molecular clusters are unevenly distributed like in Comparative Example 1, and the tensile strength decreases. In addition, due to the lack of KH550 modification, it is difficult for the powder surface to polymerize with the epoxy resin, which further reduces the elongation at break of the epoxy resin composite material.
[0129] The tear strength was tested on a Z010 universal electronic testing machine produced by Zwick / Roell of Germany according to GB / T529-2008. The examples and comparative examples were tested 5 times, and the results were averaged, as shown in Table 2.
[0130] Table 2. Tear strength table
[0131]
[0132] It can be seen that the tear strengths of the embodiments are 37.9 MPa, 36.3 MPa and 36.8 MPa, respectively, which are stronger than those of the comparative examples. The tear strength of comparative example 1 is only 10.4 MPa. The reason is the same as that of the tensile strength. In the absence of the catalyst phenol, the decomposition products are not completely decomposed, and the internal distribution of the obtained epoxy resin composite material is uneven, which reduces the overall mechanical properties of the epoxy resin composite material.
[0133] The tear strength of Comparative Example 2 is 34.2 MPa, and the tear strength of Comparative Example 3 is 31.6 MPa. In terms of tear strength, Comparative Examples 2 and 3 are not much different from the embodiment.
[0134] The Shore A hardness was measured in accordance with GB / T531-1999 standard using the LX-A rubber hardness tester produced by Wuxi Qianzhou Measuring Instrument Factory.
[0135] The above tests were performed for each sample at least five times, and the results were averaged, as shown in Table 3.
[0136] Table 3. Shore A hardness table
[0137]
[0138] As can be seen from Table 3, the Shore A hardness (HA) of the embodiments is 60 and 59, that of Comparative Example 1 is 54, and that of Comparative Example 3 is 58. Although the internal molecular distribution of Comparative Examples 1 and 3 is uneven, resulting in reduced tensile and tear properties, the hardness is mainly determined by the physical properties of the material itself. Therefore, the Shore A hardness of Comparative Examples 1 and 3 is not significantly reduced compared with that of the embodiments.
[0139] The Shore A hardness of Comparative Example 2 is 44, which is significantly lower. It is speculated that this is because the metal powder was not completely screened out, resulting in the epoxy resin composite material containing more metal impurities, which affected the physical properties and caused the hardness to decrease.
[0140] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A process for separating harmful components from degradable packaging waste and then reusing them, characterized in that: The steps include: S1: Selective dissolution and separation of metal components in degradable packaging waste The degradable packaging waste is immersed in a NaOH solution and heated to leach the metal in the waste, and then the filtrate is removed by filtering, and the filter residue is dried to obtain the treated waste, and sodium lignin sulfonate is selected as a wetting agent and mixed with pine oil to obtain a mixed solution, and the treated waste is immersed in the mixed solution for flotation, and the sedimentation part is collected and air-dried to obtain a flotation material; S2: Mixed molding of flotation material and additives The flotation material is crushed and vibrated and screened, and then fully mixed with the additive to form a mixed powder, and the mixed powder is sent to a hot press for molding to obtain a new material; S3: New materials for near-critical water decomposition Put the new material into a reactor, add distilled water, and then add a catalyst phenol, seal the reactor and put it into a salt bath furnace at 300-305°C, continue the reaction, take out the reactor after the reaction is finished, put it into cold water to quench it, collect the water phase decomposition product with a collection bottle, add ethyl acetate to the water phase decomposition product for extraction, separate the extract to obtain a solid phase product, soak the solid phase product in ethyl acetate, and then soak it in distilled water, take it out and dry it to obtain a decomposition product; S4: Surface treatment of decomposition products The decomposition product is mechanically crushed and then sieved to obtain a decomposition product powder, the decomposition product powder is added to a reaction bottle containing an ethanol solution until it is completely immersed, KH550 is added, stirred for reaction, to obtain a treatment liquid, and the treatment liquid is dried to obtain a modified powder; S5: Preparation of epoxy resin composites using modified powders Add the modified powder into a beaker containing epoxy resin, then add a defoaming agent, mechanically stir and ultrasonically disperse, to obtain intermediate I, add curing agent DDM to intermediate I, stir evenly and degas in vacuum, finally cast into a polytetrafluoroethylene mold, heat and cure in a blast drying oven to obtain intermediate II, place intermediate II in a blast drying oven and slowly cool to room temperature to obtain intermediate III, take out intermediate III from the blast drying oven, and place it for 24-26 hours to obtain an epoxy resin composite material.
2. The process for separating harmful components from degradable packaging waste and reusing them according to claim 1, characterized in that: Step S1: selectively dissolving and sorting the metal components of the degradable packaging waste, including the following steps: S1.1: Immerse the degradable packaging waste in NaOH solution for 15-20 minutes, liquid-to-solid ratio (15-20): 1, NaOH concentration 1-1.25 mol / L, raise the temperature to 60-70°C, leach the metals in the waste, then filter out the filtrate, dry the residue, and obtain the treated waste; S1.2: 6000 mg / L sodium lignin sulfonate is selected as a wetting agent, mixed with 5 mg / L pine oil to obtain a mixed solution, the treated waste is immersed in the mixed solution, and flotation is performed under the conditions of adjusting the flotation time to 15-20 min and the flotation time to 15-20 min. The sedimentation part is collected and air-dried at 60°C for 6-7 hours to obtain a flotation material.
3. The process for separating harmful components from degradable packaging waste and reusing them according to claim 2, characterized in that: Step S2: Mixing and molding the flotation material and the additive material, including the following steps: S2.1: The flotation material is crushed and vibrated for 15-20 minutes, and then fully mixed with the additive for 15-20 minutes. The mass ratio of the flotation material to the additive is (2-4):1 to form a mixed powder; S2.2: The mixed powder is sent to a hot press for compression molding. The compression pressure of the hot press is 10-12 MPa, the compression temperature is 150-160°C, and the compression time is 5-7 minutes during heating to obtain a new material.
4. The process for separating harmful components from degradable packaging waste and reusing them according to claim 3, characterized in that: Step S3, near-critical water decomposition of new materials, comprises the following steps: S3.1: Weigh and record the mass of the new material, then put the weighed new material into the reactor, add distilled water according to the material-liquid mass ratio of 1:(8-10), then add 0.2-0.5% of the total volume of catalyst phenol with a concentration of 0.4-0.7 mol / L, and seal the reactor; S3.2: Place the reactor in a salt bath furnace heated to a specified temperature of 300-305°C and continue the reaction for 45-60 minutes; S3.3: After completion, remove the reactor and place it in cold water to quench it. After leaving it for 15-20 minutes, open the reactor and collect the aqueous phase decomposition product in a collection bottle. Add ethyl acetate to the aqueous phase decomposition product for extraction. After 100-120 minutes, separate the extract to obtain a solid phase product. S3.4: Place the solid phase product in ethyl acetate, soak for 20-24 hours, and then soak in distilled water for 2-3 hours. After taking it out, dry it in an oven at a temperature of 100-110°C to obtain a decomposition product.
5. The process for separating harmful components from degradable packaging waste and reusing them according to claim 4, characterized in that: Step S4: treating the surface of the decomposition product, comprising the following steps: S4.1: The decomposition product is mechanically crushed and passed through a 200-mesh sieve to obtain a decomposition product powder, the decomposition product powder is added to a reaction bottle filled with an ethanol solution with a volume fraction of 80-95% until it is completely immersed, 1-3% of the mass of the decomposition product powder is added with KH550, and the mixture is stirred and reacted in an intelligent oil bath pot at 65-80°C for 10-12h to obtain a treated liquid; S4.2: Dry the treated liquid in a forced air drying oven at 100° C. to obtain a modified powder.
6. The process for separating harmful components from degradable packaging waste and reusing them according to claim 5, characterized in that: Step S5: preparing epoxy resin composite material by modifying powder, comprising the following steps: S5.1: Add the modified powder into a beaker containing epoxy resin, add a defoamer, stir mechanically at 65-80°C for 20-30 min, and then continue to ultrasonically disperse at 65-80°C for 50-60 min to obtain intermediate I; S5.2: Add 25-28% of the mass of intermediate I to curing agent DDM into intermediate I, stir evenly and transfer to a vacuum drying oven at 60-80°C for vacuum degassing for 8-10 minutes, and finally cast into a polytetrafluoroethylene mold preheated at 60-80°C, heat and cure in a blast drying oven, the curing conditions are 100°C for 1 hour, then 136°C for 2 hours, and finally 160°C for 1 hour, to obtain intermediate II; S5.3: Place intermediate II in a forced air drying oven and slowly cool to room temperature to obtain intermediate III; S5.4: Take out intermediate III from the forced air drying oven and leave it for 24-26 hours to obtain an epoxy resin composite material.
7. The process for separating harmful components from degradable packaging waste and reusing them according to claim 6, characterized in that: In step S1, the volume ratio of sodium lignin sulfonate to pine oil is 1:(0.5-1.5).
8. The process for separating harmful components from degradable packaging waste and reusing them according to claim 7, characterized in that: The additive in step S2 is one or more of thermosetting phenolic plastics, thermoplastic high-density polyethylene, polypropylene and polyvinyl chloride.
9. The process for separating harmful components from degradable packaging waste and reusing them according to claim 8, characterized in that: The volume ratio of the modified powder, epoxy resin and defoaming agent in step S5.1 is 1:(8-10):(1-2).
10. The process for separating harmful components from degradable packaging waste and reusing them according to claim 9, characterized in that: The defoaming agent in step S5.1 is specifically a silicone defoaming agent.