A lithium-based negative electrode material for high-rate power battery and a preparation method thereof
By using alumina gel-foam metal composite material as the skeleton for lithium alloy deposition in lithium-ion batteries, the problems of low capacity and lithium dendrites of lithium-ion batteries are solved, and high magnification and long cycle stable battery performance is achieved.
Patent Information
- Application Number
- CN202410954428.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-17
AI Technical Summary
The existing lithium-ion battery anode materials such as graphite materials have low theoretical capacity, are easy to react with electrolytes, and have lithium dendrites and volume expansion problems in high-magnification applications, making it difficult to meet the needs of fast charging and discharging and high power output.
Alumina gel-foam metal composite material is used as the skeleton deposited by lithium alloy. Through a multi-stage skeleton structure and three-dimensional cross-linking network, the formation of lithium dendrites is avoided, and the transmission efficiency of lithium ions and the cycling stability of the battery is improved.
The high capacity, long cycle stability and high rate performance of lithium-ion batteries are achieved, the formation of lithium dendrites is avoided, and the rapid charging and discharging capacity of the battery and the transmission rate of lithium ions are improved.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of negative electrode materials for new energy batteries, and in particular to a lithium-based negative electrode material for a high-rate power battery and a preparation method thereof. Background Art
[0002] With the continuous development of the new energy industry, power battery technology is also constantly improving. Traditional lead-acid batteries, manganese-zinc batteries, etc. have been unable to meet market demand due to their limited capacity and large mass volume, and lithium-ion batteries have become the mainstream power batteries. Negative electrode materials are an important factor affecting the energy density, cycle life and rate performance of lithium-ion batteries. At present, the negative electrode materials of lithium-ion batteries can be mainly divided into two categories: carbon-based and non-carbon-based. Carbon-based materials include natural graphite, artificial graphite, soft carbon, and hard carbon; non-carbon-based materials include silicon-based materials (silicon oxygen, silicon carbon, silicon-based alloys), lithium titanate, tin-based materials, etc. Compared with the situation in which lithium iron phosphate and ternary materials compete with each other in the field of positive electrode materials, the technical route of negative electrode materials is relatively single. Artificial graphite has always occupied an absolute mainstream position in the lithium battery negative electrode material market, with a market share of over 80%. However, as a common negative electrode material, graphite material has a theoretical capacity of only 372mAh / g, a low acceptance capacity for lithium ions, and poor compatibility with organic solvents, which makes it easy to react with the electrolyte and reduce the ability to deintercalate lithium ions. In order to adapt to the new requirements brought about by scientific and technological progress, lithium-ion batteries, especially electrode materials, are in urgent need of new breakthroughs.
[0003] Lithium metal has an extremely high theoretical specific capacity of 3860mAh / g, which is 10 times that of commercial graphite negative electrodes. This means that if lithium metal can be effectively used as a negative electrode material, the energy density of lithium-ion batteries will be greatly improved. However, due to the volume expansion and lithium dendrite growth of lithium metal negative electrodes during long-term cyclic use, it is obviously not practical to directly use lithium metal negative electrodes. For this reason, researchers have developed a series of lithium-based negative electrode materials, such as lithium alloy negative electrode materials, lithium titanate composite negative electrode materials, lithium silicon composite negative electrode materials, etc.
[0004] High-rate batteries are widely used in electric vehicles, drones, power tools and other fields. These fields have high requirements for battery power density and charge and discharge speed, and high-rate batteries are needed to meet the needs of fast charge and discharge and high power output. It can be seen that how to improve the rate of power batteries is a research technology direction required by the market. Summary of the invention
[0005] In order to solve the problems mentioned in the background technology, the present invention provides a lithium-based negative electrode material for a high-rate power battery, which adopts alumina gel-foam metal as a skeleton and deposits lithium alloy on the skeleton, thereby achieving uniform, minimal expansion, and dendrite-free deposition of lithium. While being used in power batteries to maintain high capacity, it can also improve cycle stability and rate performance.
[0006] Specifically:
[0007] A method for preparing a lithium-based negative electrode material for a high-rate power battery, the steps comprising:
[0008] Step 1, pre-treating the foam metal for standby use;
[0009] Step 2, dissolving aluminum chloride hexahydrate in a mixed solvent of ethanol and water and stirring to react, and obtaining an alumina sol after the reaction is completed;
[0010] Step 3, impregnating the foamed metal with alumina sol, taking it out and placing it in a constant temperature drying oven to increase the temperature for gelation reaction, repeating the impregnation and gelation reaction several times, and then performing supercritical drying to avoid shrinkage and cracking of the gel during the drying process, and then calcining to remove residual organic matter, enhance the crystallinity and mechanical strength of the aerogel, and obtain an alumina gel-foamed metal composite material;
[0011] Step 4: melt the lithium-aluminum alloy, and then immerse the alumina gel-foam metal composite material obtained in step 3 into the molten lithium-aluminum alloy liquid, take it out and cool it, and obtain the lithium-based negative electrode material through post-processing.
[0012] When implementing the above embodiment, preferably, the foam metal pretreatment process of step 1 includes: cleaning the foam metal with ethanol to remove surface oil and impurities, then performing ultrasonic cleaning to further clean the microporous structure of the foam nickel, and drying to ensure that there is no moisture on its surface;
[0013] When implementing the above embodiment, preferably, the foam metal in step 1 is foam nickel.
[0014] When implementing the above embodiment, preferably, in step 2, the molar ratio of aluminum chloride hexahydrate to ethanol and water is 1:6-8:13-15.
[0015] When implementing the above embodiment, preferably, the reaction in step 2 is carried out at 40-50° C., the pH is adjusted to 3-4, and the reaction time is 2-5 h.
[0016] When implementing the above embodiment, preferably, in step 3, the time for impregnation of the foam metal with the alumina sol is 10-20 minutes; the constant temperature drying oven is heated to 70-80° C., and the gelation reaction time is 5-10 hours; and the impregnation and gelation reactions are repeated 2-3 times.
[0017] When implementing the above embodiment, preferably, the medium for supercritical drying in step 3 is carbon dioxide in a supercritical state; the roasting temperature is 700-800° C., and the roasting time is 0.5-1 h.
[0018] When implementing the above embodiment, preferably, in step 4, the time for impregnating the alumina gel-foam metal composite material with the molten lithium-aluminum alloy is 2-3 minutes.
[0019] When implementing the above embodiment, preferably, the post-processing process in step 4 includes cleaning and drying.
[0020] On the other hand, the present invention provides a lithium-based negative electrode material for a high-rate power battery, which is prepared by the above-mentioned preparation method.
[0021] Compared with the prior art, the present invention has the following beneficial features:
[0022] 1. The lithium-based negative electrode material of the present invention uses cheap and readily available foam metal and constructs an alumina gel network in the pores of the foam metal to form a multi-level skeleton structure as a skeleton for lithium alloy deposition; the empty space inside the foam metal is relatively large, which results in the large-sized voids still being an original lithium deposition and peeling environment, and lithium dendrite defects will still exist in these internal pores during the long-term cycle of the battery, and small-sized modified particles may detach and peel off. For this reason, the present invention combines the foam metal with the alumina gel framework to construct a three-dimensional cross-linked network structure, and the alumina gel will fill the large-sized pores inside the foam metal, and the synergistic effect of the two is used to solve the above-mentioned defects.
[0023] 2. The lithium-based negative electrode material of the present invention uses alumina gel-foam metal as a skeleton, and uses the porous structure of the two to provide a channel for the transmission of lithium ions. The high porosity of the material provides a large amount of effective lithium storage space. At the same time, the ultra-high lithium ion diffusion rate of the lithium-aluminum alloy itself can quickly transmit the accumulated lithium ion flow, which can not only improve the battery's ability to charge and discharge quickly in a short period of time, but also avoid the tip effect caused by lithium ion accumulation, thereby slowing down the formation of lithium dendrites.
[0024] 3. The lithium-based negative electrode material of the present invention constructs a structure of lithium alloy combined with a special skeleton to reduce the lithium nucleation barrier and increase the lithium ion transfer rate, thereby preparing a dendrite-free, high-rate, and long-cycle lithium-based negative electrode material. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] In order to facilitate those skilled in the art to implement the present invention, some of the reagents used in the embodiments and comparative examples are now described:
[0027] Foam metal: nickel foam, Suzhou Dekun Electronic Technology;
[0028] Aluminum chloride hexahydrate: Shanghai Gaoming Chemical;
[0029] Ethanol: Shandong Huayu Chemical;
[0030] Lithium aluminum alloy: content ≥99%, Shanghai Longjin Metal Materials;
[0031] Artificial graphite negative electrode material: BYD New Materials. Example 1
[0032] A lithium-based negative electrode material is prepared by the following preparation method:
[0033] Step 1: Use ethanol to clean the 2×5 cm nickel foam with a thickness of 0.3 mm, then perform ultrasonic deep cleaning, and then dry it for standby use;
[0034] Step 2, dissolving aluminum chloride hexahydrate in a mixed solvent of ethanol and water at a molar ratio of aluminum chloride hexahydrate to ethanol and water of 1:6:15, stirring and reacting at 40° C. and a pH value of 3 for 2 hours, and obtaining an alumina sol after the reaction is completed;
[0035] Step 3, impregnating the foamed metal with alumina sol for 10 minutes, taking it out and placing it in a constant temperature drying oven and heating it to 70°C for gelation reaction, and the reaction time is 10 hours; repeating the impregnation and gelation reaction twice; then placing it in a supercritical carbon dioxide autoclave for drying, and then calcining it at a calcination temperature of 700°C for 1 hour to obtain an alumina gel-foamed metal composite material;
[0036] Step 4: melt the lithium-aluminum alloy and control the temperature at 730°C. Then immerse the alumina gel-foam metal composite material obtained in step 3 in the molten lithium-aluminum alloy for 2 minutes. After taking it out, use a suitable solvent ethanol to wash and dry it to obtain a lithium-based negative electrode material. Example 2
[0037] A lithium-based negative electrode material is prepared by the following preparation method:
[0038] Step 1: Use ethanol to clean the 2×5 cm nickel foam with a thickness of 0.3 mm, then perform ultrasonic deep cleaning, and then dry it for standby use;
[0039] Step 2, dissolving aluminum chloride hexahydrate in a mixed solvent of ethanol and water at a molar ratio of aluminum chloride hexahydrate to ethanol and water of 1:8:13, stirring and reacting at 50° C. and a pH value of 4 for 5 hours, and obtaining an alumina sol after the reaction is completed;
[0040] Step 3, impregnating the foamed metal with alumina sol for 20 minutes, taking it out and placing it in a constant temperature drying oven and heating it to 80°C for gelation reaction, and the reaction time is 5 hours; repeating the impregnation and gelation reaction 3 times; then placing it in a supercritical carbon dioxide autoclave for drying, and then calcining it at a calcination temperature of 800°C and a calcination time of 0.5 hours to obtain an alumina gel-foamed metal composite material;
[0041] Step 4: melt the lithium-aluminum alloy and control the temperature at 740°C. Then immerse the alumina gel-foam metal composite material obtained in step 3 in the molten lithium-aluminum alloy for 3 minutes. After taking it out, use a suitable solvent ethanol to wash and dry it to obtain a lithium-based negative electrode material. Example 3
[0042] A lithium-based negative electrode material is prepared by the following preparation method:
[0043] Step 1: Use ethanol to clean the 2×5 cm nickel foam with a thickness of 0.3 mm, then perform ultrasonic deep cleaning, and then dry it for standby use;
[0044] Step 2, dissolving aluminum chloride hexahydrate in a mixed solvent of ethanol and water at a molar ratio of aluminum chloride hexahydrate to ethanol and water of 1:7:13, stirring and reacting at 40° C. and a pH value of 3.5 for 3.5 hours, and obtaining an alumina sol after the reaction is completed;
[0045] Step 3, impregnating the foamed metal with alumina sol for 15 minutes, taking it out and placing it in a constant temperature drying oven and heating it to 75°C for gelation reaction, and the reaction time is 6 hours; repeating the impregnation and gelation reaction 3 times; then placing it in a supercritical carbon dioxide autoclave for drying, and then calcining it at a calcination temperature of 720°C and a calcination time of 0.5 hours to obtain an alumina gel-foamed metal composite material;
[0046] Step 4: melt the lithium-aluminum alloy and control the temperature at 730°C. Then immerse the alumina gel-foam metal composite material obtained in step 3 in the molten lithium-aluminum alloy for 2 minutes. After taking it out, use a suitable solvent ethanol to wash and dry it to obtain a lithium-based negative electrode material. Example 4
[0047] A lithium-based negative electrode material is prepared by the following preparation method:
[0048] Step 1: Use ethanol to clean the 2×5 cm nickel foam with a thickness of 0.3 mm, then perform ultrasonic deep cleaning, and then dry it for standby use;
[0049] Step 2, dissolving aluminum chloride hexahydrate in a mixed solvent of ethanol and water at a molar ratio of aluminum chloride hexahydrate to ethanol and water of 1:8:14, stirring and reacting at 45° C. and a pH value of 3-4 for 4 hours, and obtaining an alumina sol after the reaction is completed;
[0050] Step 3, impregnating the foamed metal with alumina sol for 20 minutes, taking it out and placing it in a constant temperature drying oven and heating it to 78°C for gelation reaction, and the reaction time is 8 hours; repeating the impregnation and gelation reaction 3 times; then placing it in a supercritical carbon dioxide autoclave for drying, and then calcining it at a calcination temperature of 780°C and a calcination time of 0.8 hours to obtain an alumina gel-foamed metal composite material;
[0051] Step 4: melt the lithium-aluminum alloy and control the temperature at 735°C. Then immerse the alumina gel-foam metal composite material obtained in step 3 in the molten lithium-aluminum alloy for 2 minutes. After taking it out, use a suitable solvent ethanol to wash and dry it to obtain a lithium-based negative electrode material. Example 5
[0052] A lithium-based negative electrode material is prepared by the following preparation method:
[0053] Step 1: Use ethanol to clean the 2×5 cm nickel foam with a thickness of 0.3 mm, then perform ultrasonic deep cleaning, and then dry it for standby use;
[0054] Step 2, dissolving aluminum chloride hexahydrate in a mixed solvent of ethanol and water at a molar ratio of aluminum chloride hexahydrate to ethanol and water of 1:6:13, stirring and reacting at 43° C. and a pH value of 3.5 for 3 hours, and obtaining an alumina sol after the reaction is completed;
[0055] Step 3, impregnating the foamed metal with alumina sol for 12 minutes, taking it out and placing it in a constant temperature drying oven and heating it to 74°C for gelation reaction, and the reaction time is 6 hours; repeating the impregnation and gelation reaction 3 times; then placing it in a supercritical carbon dioxide autoclave for drying, and then calcining it at a calcination temperature of 730°C and a calcination time of 0.8 hours to obtain an alumina gel-foamed metal composite material;
[0056] Step 4: melt the lithium-aluminum alloy and control the temperature at 740°C. Then immerse the alumina gel-foam metal composite material obtained in step 3 in the molten lithium-aluminum alloy for 2 minutes. After taking it out, use a suitable solvent ethanol to wash and dry it to obtain a lithium-based negative electrode material.
[0057] Comparative Example 1
[0058] Artificial graphite negative electrode material is used.
[0059] Performance Testing:
[0060] (1) Preparation of batteries with lithium-based negative electrode materials of Examples 1-5: The lithium-based negative electrode materials prepared in each example were placed in a glove box. The lithium-based negative electrode materials were placed on the negative electrode side, the lithium sheet was placed on the positive electrode side, and PE was used as a separator to assemble into a button half-cell.
[0061] (2) Preparation of a battery using the artificial graphite negative electrode material of Comparative Example 1: Using N-methylpyrrolidone as a solvent, adding artificial graphite negative electrode material, conductive carbon black, and binder LA132, the amount ratio of artificial graphite negative electrode material: conductive carbon black: LA132: solvent is 90 g: 1 g: 5 g: 200 mL, stirring to make a slurry and coating it on a copper foil, and then drying and rolling to obtain a negative electrode; the electrolyte is a mixture of ethylene carbonate (EC) / diethyl carbonate (DEC) / ethyl methyl carbonate (EMC) containing 1 mol / L LiPF6 (the volume ratio of EC, DEC and EMC is 1:1:1); the metal lithium sheet is the counter electrode; the diaphragm is a polypropylene (PP) film; and the button half-cell is assembled in an argon-filled glove box.
[0062] Each group of batteries prepared above was tested on the LAND battery testing system. The test results are shown in the following table:
[0063] 5C discharge capacity retention rate / % 10C, 1000 charge and discharge cycles, discharge capacity retention rate / % Example 1 96.02 92.08 Example 2 96.54 94.32 Example 3 95.97 90.59 Example 4 95.38 91.33 Example 5 96.16 92.81 Comparative Example 1 84.69 80.15
[0064] It can be seen from the above experimental data that the two groups of test data of Examples 1-5 at 5C discharge capacity retention rate and 10C, 1000 charge and discharge times, discharge capacity retention rate are much higher than those of Comparative Example 1, which proves that the lithium-based negative electrode material used in the present invention has high rate performance and the discharge capacity is still good under long cycles.
[0065] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a lithium-based negative electrode material for a high-rate power battery, characterized in that: The steps include: Step 1, pre-treating the foam metal for standby use; the foam metal is selected from foam nickel; Step 2, dissolving aluminum chloride hexahydrate in a mixed solvent of ethanol and water and stirring to react, and obtaining an alumina sol after the reaction is completed; Step 3, impregnating the foamed metal with alumina sol, taking it out and placing it in a constant temperature drying oven to increase the temperature for gelation reaction, repeating the impregnation and gelation reaction several times, and then performing supercritical drying and calcination to obtain an alumina gel-foamed metal composite material; Step 4: melt the lithium-aluminum alloy, and then immerse the alumina gel-foam metal composite material obtained in step 3 into the molten lithium-aluminum alloy liquid, take it out and cool it, and obtain the lithium-based negative electrode material through post-processing.
2. The method for preparing a lithium-based negative electrode material for a high-rate power battery according to claim 1, characterized in that: The foam metal pretreatment process of step 1 includes: cleaning the foam metal with ethanol, then performing ultrasonic cleaning, and drying.
3. The method for preparing a lithium-based negative electrode material for a high-rate power battery according to claim 1, characterized in that: In step 2, the molar ratio of aluminum chloride hexahydrate to ethanol and water is 1:6-8:13-15.
4. The method for preparing a lithium-based negative electrode material for a high-rate power battery according to claim 3, characterized in that: The reaction in step 2 is carried out at 40-50° C., the pH is adjusted to 3-4, and the reaction time is 2-5 hours.
5. The method for preparing a lithium-based negative electrode material for a high-rate power battery according to claim 1, characterized in that: In step 3, the time for impregnating the foam metal with the alumina sol is 10-20 minutes; the temperature of the constant temperature drying oven is raised to 70-80° C., and the gelation reaction time is 5-10 hours; and the impregnation and gelation reactions are repeated 2-3 times.
6. The method for preparing a lithium-based negative electrode material for a high-rate power battery according to claim 1, characterized in that: In step 3, the medium for supercritical drying is carbon dioxide in a supercritical state; the calcination temperature is 700-800° C., and the calcination time is 0.5-1 h.
7. The method for preparing a lithium-based negative electrode material for a high-rate power battery according to claim 1, characterized in that: In step 4, the time for impregnating the alumina gel-foam metal composite material with the molten lithium-aluminum alloy is 2-3 minutes.
8. The method for preparing a lithium-based negative electrode material for a high-rate power battery according to claim 1, characterized in that: The post-processing process in step 4 includes cleaning and drying.
9. A lithium-based negative electrode material for a high-rate power battery, characterized in that: The method is prepared by any one of claims 1 to 8.