Environmentally friendly flame-retardant composite fabric and preparation process thereof
By combining modified graphite particles with polyurethane hot melt adhesive in flame-retardant composite fabrics, the problems of environmental pollution and reduced breathability of traditional flame-retardant fabrics have been solved, achieving an improvement in both environmentally friendly flame-retardant performance and breathability.
Patent Information
- Application Number
- CN202410728200.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-06-06
AI Technical Summary
Existing flame-retardant fabrics have a significant environmental impact when using halogenated flame retardants, and the breathability of multi-layer composite fabrics is significantly reduced.
Modified graphite particles are combined with polyurethane hot melt adhesive to form an environmentally friendly flame-retardant composite fabric. During the hot pressing process, the modified graphite particles expand and embed into the pores of the fabric base and the lining base, improving the flame-retardant performance. Breathability is improved by controlling the porosity and uniform thickness distribution.
It achieves improved environmentally friendly flame-retardant performance while maintaining the breathability of the fabric, thus solving the environmental pollution problem caused by traditional flame-retardant fabrics.
Smart Images

Figure BDA0004879366420000071 
Figure BDA0004879366420000081
Abstract
Description
Technical Field
[0001] The invention relates to the field of textiles, and in particular to an environmentally friendly flame-retardant composite fabric and a preparation process thereof. Background Art
[0002] Fabrics are materials used to make clothing. As one of the three elements of clothing, fabrics can not only interpret the style and characteristics of clothing, but also directly affect the color and shape of clothing. Flame-retardant fabrics are made of flame-retardant fibers. They can only smolder in flames without emitting flames themselves. When leaving the flame, the smoldering will go out by itself. They are widely used in clothing, home furnishings, decorations, non-woven fabrics and fillings. Existing flame-retardant fabrics are usually used as outer surfaces, but existing multi-layer composite fabrics are often added with halogen flame retardants when flame-retardant, which has a greater impact on the environment. In addition, the air permeability of multi-layer fabrics is significantly reduced during the glue compounding process. Summary of the invention
[0003] The object of the present invention is to provide an environmentally friendly flame-retardant composite fabric and a preparation process thereof, so as to solve the problems raised in the above background technology.
[0004] According to a first aspect of the present invention, an environmentally friendly flame-retardant composite fabric is provided, which mainly comprises the following raw material components in parts by weight: 90 parts of fabric base fabric, 70 parts of lining base fabric and 40 parts of flame-retardant hot-melt adhesive, wherein the fabric base fabric and the lining base fabric are hot-melt bonded by the flame-retardant hot-melt adhesive to form the environmentally friendly flame-retardant composite fabric; the flame-retardant hot-melt adhesive mainly comprises polyurethane hot-melt adhesive and modified graphite particles, and the modified graphite particles are prepared from expanded graphite and natural graphite; the thickness of the fabric base fabric is h1, and the porosity is a; the thickness of the lining base fabric is h2, and the porosity is b, wherein h1, a, h2, and b satisfy the relationship 2.0≤(h1-h2) / (ab)≤8.5.
[0005] When preparing the environmentally friendly flame-retardant composite fabric, the present invention adds modified graphite particles to the middle hot melt adhesive layer. Since the modified graphite particles expand during the hot pressing process, the expanded graphite can be partially embedded in the pores of the fabric base cloth and the lining base cloth of the composite fabric, thereby blocking the direct contact between the open flame and the fabric during combustion, promoting the carbonization of the fabric, and improving the flame retardant performance of the fabric in vertical combustion. At the same time, the porosity and thickness of the fabric base cloth and the lining base cloth are controlled, so that the modified graphite particles can be evenly embedded in the fabric base cloth and the lining base cloth, thereby improving the lateral flame retardant performance of the composite fabric. At the same time, since the European graphite forms abundant pores after expansion and is evenly distributed in the pores of the fabric base cloth and the lining base cloth, the air permeability of the fabric can be improved.
[0006] In a second aspect, the present invention provides a process for preparing an environmentally friendly flame-retardant composite fabric, comprising the following steps:
[0007] (1) selecting a fabric base fabric and a lining base fabric, respectively performing a slurry treatment on the fabric base fabric and the lining base fabric through a slurry impregnation machine, and then drying to obtain a pretreated fabric base fabric and a pretreated lining base fabric;
[0008] (2) mixing the pretreated fabric base fabric and the pretreated lining base fabric with an acetic acid aqueous solution having a concentration of 3 to 10%, filtering, and washing with water until the washing liquid is neutral to obtain a fabric base fabric blank and a lining base fabric blank;
[0009] (3) Take 90 parts of the fabric base fabric blank obtained in step (2), 70 parts of the lining base fabric blank obtained in step (2) and 40 parts of the flame retardant hot melt adhesive in sequence, by weight, apply the flame retardant hot melt adhesive on one side of the lining base fabric blank, and composite the fabric base fabric blank on the flame retardant hot melt adhesive, and heat-press and cure them to obtain an environmentally friendly flame retardant composite fabric.
[0010] When preparing the environmentally friendly flame-retardant composite fabric, the present invention first uses a slurry containing nano calcium carbonate to perform a slurry treatment on the fabric base fabric and the lining base fabric, and then uses acetic acid to treat it, which can improve the porosity of the fabric base fabric and the lining base fabric to a certain extent, so that when the fabric base fabric and the lining base fabric are subsequently bonded with hot-melt adhesive, the hot-melt adhesive penetrates into the pores of the fabric base fabric and the lining base fabric, thereby improving the air permeability of the product. DETAILED DESCRIPTION
[0011] According to a first aspect of the present invention, an environmentally friendly flame-retardant composite fabric is provided, which mainly comprises the following raw material components in parts by weight: 90 parts of fabric base fabric, 70 parts of lining base fabric and 40 parts of flame-retardant hot-melt adhesive, wherein the fabric base fabric and the lining base fabric are hot-melt bonded by the flame-retardant hot-melt adhesive to form the environmentally friendly flame-retardant composite fabric; the flame-retardant hot-melt adhesive mainly comprises polyurethane hot-melt adhesive and modified graphite particles, and the modified graphite particles are prepared from expanded graphite and natural graphite; the thickness of the fabric base fabric is h1, and the porosity is a; the thickness of the lining base fabric is h2, and the porosity is b, wherein h1, a, h2, and b satisfy the relationship 2.0≤(h1-h2) / (ab)≤8.5.
[0012] Preferably, the range of h1-h2 is 0.2 mm to 1.8 mm, the range of h1 is 0.3 to 2.0 mm, and the range of h2 is 0.1 to 1.2 mm.
[0013] Preferably, ab is in the range of 0.10 to 0.28, a is in the range of 0.25 to 0.50, and b is in the range of 0.15 to 0.30.
[0014] Preferably, the modified graphite particles are prepared by mixing expanded graphite and natural graphite and then mixing with water to prepare a dispersion with a mass fraction of 5 to 20%, and then spray-drying to obtain modified graphite particles with a particle size of 100 to 500 μm.
[0015] Preferably, the mass ratio of the expanded graphite to the natural graphite in the modified graphite particles is 1:2 to 1:4.
[0016] Preferably, the outer fabric base fabric and the lining base fabric are each selected from any one of polyester fabric, polypropylene fabric, acrylic fabric or nylon fabric.
[0017] In a second aspect, the present invention provides a process for preparing an environmentally friendly flame-retardant composite fabric, comprising the following steps:
[0018] (1) selecting a fabric base fabric and a lining base fabric, respectively performing a slurry treatment on the fabric base fabric and the lining base fabric through a slurry impregnation machine, and then drying the slurry to obtain a pretreated fabric base fabric and a pretreated lining base fabric;
[0019] (2) mixing the pretreated fabric base fabric and the pretreated lining base fabric with an acetic acid aqueous solution having a concentration of 3 to 10%, filtering, and washing with water until the washing liquid is neutral to obtain a fabric base fabric blank and a lining base fabric blank;
[0020] (3) Take 90 parts of the fabric base fabric blank obtained in step (2), 70 parts of the lining base fabric blank obtained in step (2) and 40 parts of the flame retardant hot melt adhesive in sequence, by weight, apply the flame retardant hot melt adhesive on one side of the lining base fabric blank, and composite the fabric base fabric blank on the flame retardant hot melt adhesive, and heat-press and cure them to obtain an environmentally friendly flame retardant composite fabric.
[0021] Preferably, the preparation method of the slurry used for the slurry treatment in step (1) is to mix 50 parts of a 30% to 50% aqueous acrylic emulsion by mass, 30 parts of water, 3 parts of a penetrant JFC, 3.5 parts of 40% ammonia water and 8 parts of nano calcium carbonate to obtain the slurry used for slurry treatment.
[0022] Preferably, the slurry treatment in step (1) is carried out at a temperature of 60 to 100° C. and a pressure of 2 to 3 MPa.
[0023] Preferably, the hot pressing curing conditions in step (3) are first hot pressing for 30 seconds at a temperature of 250-300°C and a pressure of 3-8 MPa, and then hot pressing for 1-2 hours at a temperature of 50°C and a pressure of 2-5 MPa.
[0024] Example 1
[0025] An environmentally friendly flame-retardant composite fabric, measured by weight, mainly includes:
[0026] 90 parts of fabric base cloth, 70 parts of lining base cloth and 40 parts of flame retardant hot melt adhesive, wherein the fabric base cloth and the lining base cloth are both polyester cloth, wherein the thickness h1 of the fabric base cloth is 1.2 mm, and the porosity a is 30%; the thickness h2 of the lining base cloth is 0.4 mm, and the porosity b is 16%, and the particle size of the modified graphite particles in the flame retardant hot melt adhesive is 200 μm, and the content is 20%.
[0027] An environmentally friendly flame-retardant composite fabric comprises the following steps:
[0028] (1) Selecting a fabric base fabric and a lining base fabric, weighing in parts by weight: 50 parts of a 40% aqueous acrylic emulsion, 30 parts of water, 3 parts of a penetrant JFC, 3.5 parts of a 40% ammonia water and 8 parts of nano calcium carbonate, stirring and mixing to obtain a slurry for slurrying, adding the slurry for slurrying to a slurrying machine, and slurrying the fabric base fabric and the lining base fabric for 2 hours at a temperature of 70° C. and a pressure of 2.5 MPa, and drying them at a temperature of 80° C. for 3 hours to obtain a pretreated fabric base fabric and a pretreated lining base fabric;
[0029] (2) The pretreated fabric base fabric and the pretreated lining base fabric were respectively mixed with a 7% acetic acid aqueous solution at a mass ratio of 1:10, and then the mixture was soaked at room temperature for 3 hours and filtered to obtain a filter cake. The filter cake was washed with water until the washing liquid was neutral and then dried at a temperature of 60° C. to constant weight to obtain a fabric base fabric blank and a lining base fabric blank;
[0030] (3) According to the weight ratio, 90 parts of the fabric base fabric blank obtained in step (2), 70 parts of the lining base fabric blank obtained in step (2) and 40 parts of the flame retardant hot melt adhesive are taken in sequence, the flame retardant hot melt adhesive is applied to one side of the lining base fabric blank, and the fabric base fabric blank is composited on the flame retardant hot melt adhesive, firstly hot pressed at a temperature of 280°C and a pressure of 5 MPa for 30 seconds, and then hot pressed and cured at a temperature of 50°C and a pressure of 3 MPa for 1.5 hours to obtain an environmentally friendly flame retardant composite fabric.
[0031] Example 2
[0032] The difference between Example 2 and Example 1 is that the thickness h1 of the outer fabric base cloth is 1.9 mm, and the porosity a is 40%; the thickness h2 of the lining base cloth is 0.1 mm, and the porosity b is 15%.
[0033] The remaining steps are the same as those in Example 1.
[0034] Example 3
[0035] The difference between Example 3 and Example 1 is that the thickness h1 of the outer fabric base cloth is 0.3 mm, and the porosity a is 25%; the thickness h2 of the lining base cloth is 0.1 mm, and the porosity b is 15%.
[0036] The remaining steps are the same as those in Example 1.
[0037] Example 4
[0038] The difference between Example 4 and Example 1 is that the thickness h1 of the outer fabric base cloth is 0.8 mm, and the porosity a is 28%; the thickness h2 of the lining base cloth is 0.75 mm, and the porosity b is 26%.
[0039] The remaining steps are the same as those in Example 1.
[0040] Example 5
[0041] The difference between Example 5 and Example 1 is that the thickness h1 of the outer fabric base cloth is 2 mm, and the porosity a is 40%; the thickness h2 of the lining base cloth is 0.15 mm, and the porosity b is 15%.
[0042] The remaining steps are the same as those in Example 1.
[0043] Example 6
[0044] The difference between Example 6 and Example 1 is that the thickness h1 of the outer fabric base cloth is 1.3 mm, and the porosity a is 25%; the thickness h2 of the lining base cloth is 0.6 mm, and the porosity b is 16%.
[0045] The remaining steps are the same as those in Example 1.
[0046] Example 7
[0047] The difference between Example 7 and Example 1 is that the thickness h1 of the outer fabric base cloth is 1.5 mm, and the porosity a is 50%; the thickness h2 of the lining base cloth is 0.7 mm, and the porosity b is 20%.
[0048] The remaining steps are the same as those in Example 1.
[0049] Comparative Example 1
[0050] The difference between Comparative Example 1 and Example 1 is that the thickness h1 of the outer fabric base cloth is 1.5 mm, and the porosity a is 32%; the thickness h2 of the lining base cloth is 1.3 mm, and the porosity b is 21%.
[0051] The remaining steps are the same as those in Example 1.
[0052] Comparative Example 2
[0053] The difference between Comparative Example 1 and Example 1 is that the thickness h1 of the outer fabric base cloth is 1.9 mm, and the porosity a is 47%; the thickness h2 of the lining base cloth is 0.3 mm, and the porosity b is 28%.
[0054] The remaining steps are the same as those in Example 1.
[0055] Comparative Example 3
[0056] The difference between Comparative Example 3 and Example 1 is that the thickness h1 of the outer fabric base is 1.2 mm, and the porosity a is 30%; the thickness h2 of the lining base is 0.5 mm, and the porosity b is 17%. In addition, in step (1), nano calcium carbonate is not added to the slurry used for slurry dipping.
[0057] The remaining steps are the same as those in Example 1.
[0058] Comparative Example 4
[0059] The difference between Comparative Example 4 and Example 1 is that the thickness h1 of the outer fabric base cloth is 1.3 mm, and the porosity a is 30%; the thickness h2 of the lining base cloth is 0.5 mm, and the porosity b is 14%. At the same time, in step (3), no modified graphite particles are added to the flame retardant hot melt adhesive, and only natural graphite particles with a particle size of 200 μm are added, and the addition amount is 20%.
[0060] The remaining steps are the same as those in Example 1.
[0061] Test Case
[0062] (1) Flame retardant performance test
[0063] The horizontal burning rate of the products obtained from Examples 1 to 7 and Comparative Examples 1 to 4 was tested according to standard GB8410, the vertical burning rate of the products obtained from Examples 1 to 7 and Comparative Examples 1 to 4 was tested according to standard GB32086, and the limiting oxygen index of the products obtained from Examples 1 to 7 and Comparative Examples 1 to 4 was tested according to standard GB / T5454. The specific test results are shown in Table 1.
[0064] (2) Air permeability test
[0065] The air permeability of the products obtained in Examples 1 to 7 and Comparative Examples 1 to 4 was tested according to standard GB / T5453. The specific test results are shown in Table 1.
[0066] Table 1 Flame retardant properties and air permeability test results of the environmentally friendly flame retardant composite fabrics obtained in Examples 1-7 and Comparative Examples 1-4
[0067]
[0068]
[0069] Through the test data of the products obtained from Examples 1 to 7 and Comparative Examples 1 to 4 in Table 1, it can be found that when modified graphite particles are added to the flame-retardant hot melt adhesive used in the product, and the thickness and porosity of the fabric base cloth and the lining base cloth are controlled within a certain ratio, the product can have good air permeability and flame retardant properties.
[0070] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. An environmentally friendly flame-retardant composite fabric, characterized in that: The invention mainly comprises the following raw material components in parts by weight: 90 parts of fabric base cloth, 70 parts of lining base cloth and 40 parts of flame retardant hot melt adhesive, wherein the fabric base cloth and the lining base cloth are hot-melt bonded by the flame retardant hot melt adhesive to form the environmentally friendly flame retardant composite fabric; the flame retardant hot melt adhesive mainly comprises polyurethane hot melt adhesive and modified graphite particles, and the modified graphite particles are prepared from expanded graphite and natural graphite; the thickness of the fabric base cloth is h1, and the porosity is a; the thickness of the lining base cloth is h2, and the porosity is b, wherein h1, a, h2, and b satisfy the relationship 2.0≤(h1-h2) / (ab)≤8.5; The range of h1-h2 is 0.2mm~1.8mm, the range of h1 is 0.3~2.0mm, and the range of h2 is 0.1~1.2mm; The range of ab is 0.10-0.28, the range of a is 0.25-0.50, and the range of b is 0.15-0.30; The modified graphite particles are prepared by mixing expanded graphite and natural graphite, and then mixing with water to prepare a dispersion with a mass fraction of 5-20%, and then spray drying to obtain modified graphite particles with a particle size of 100-500 μm; The mass ratio of the expanded graphite to the natural graphite in the modified graphite particles is 1:2 to 1:4; The fabric base fabric and the lining base fabric are each selected from any one of polyester fabric, polypropylene fabric, acrylic fabric or nylon fabric; The environmentally friendly flame-retardant composite fabric is mainly prepared by the following steps: (1) Selecting a fabric base fabric and a lining base fabric, respectively performing slurry treatment on the fabric base fabric and the lining base fabric through a slurry impregnation machine, and then drying to obtain a pretreated fabric base fabric and a pretreated lining base fabric; (2) The pretreated fabric base fabric and the pretreated lining base fabric are respectively mixed with an acetic acid aqueous solution with a concentration of 3-10%, filtered, and washed with water until the washing liquid is neutral to obtain a fabric base fabric blank and a lining base fabric blank; (3) Taking 80-100 parts of the fabric base fabric blank obtained in step (2), 70-90 parts of the lining base fabric blank obtained in step (2) and 30-50 parts of the flame retardant hot melt adhesive in order by weight, applying the flame retardant hot melt adhesive on one side of the lining base fabric blank, and compounding the fabric base fabric blank on the flame retardant hot melt adhesive, and hot pressing and curing, to obtain an environmentally friendly flame retardant composite fabric.
2. The environmentally friendly flame-retardant composite fabric according to claim 1, characterized in that: The preparation method of the slurry used for the slurry treatment in step (1) is to mix 50 parts of an aqueous acrylic emulsion with a mass fraction of 30% to 50%, 30 parts of water, 3 parts of a penetrant JFC, 3.5 parts of ammonia water with a concentration of 40% and 8 parts of nano calcium carbonate to obtain the slurry used for slurry treatment.
3. The environmentally friendly flame-retardant composite fabric according to claim 1, characterized in that: The conditions for the slurry treatment in step (1) are to carry out the slurry treatment at a temperature of 60-100° C. and a pressure of 2-3 MPa.
4. The environmentally friendly flame-retardant composite fabric according to claim 1, characterized in that: The hot pressing curing conditions of step (3) are: first hot pressing for 30 seconds at a temperature of 250-300°C and a pressure of 3-8 MPa, and then hot pressing for 1-2 hours at a temperature of 50°C and a pressure of 2-5 MPa.