A method for preparing modified fiber-reinforced alumina ceramics
By coating modified alumina fibers with lithium galvanic stone and combining sintering additives, the brittleness and thermal expansion problems of alumina ceramic materials are solved, and its bending strength, fracture toughness and thermal shock resistance are significantly improved.
Patent Information
- Application Number
- CN202410641676.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-22
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-05-22
AI Technical Summary
Alumina ceramic materials have high brittleness and poor toughness, high thermal expansion coefficient and low thermal conductivity, which leads to prone to rupture at high temperatures, limiting their widespread application.
Modified alumina fibers are coated with lithium cylindrical stone, and ball milled with alumina powder and sintering aids, and modified fiber toughened alumina ceramics are prepared by drying, granulating, pressing molding and sintering.
The bending strength and fracture toughness of alumina ceramics are significantly improved, and their thermal shock resistance is improved, so that they exhibit excellent mechanical properties and high temperature stability at high temperatures.
Smart Images

Figure CN118495973B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of ceramic materials, and in particular to a method for preparing modified fiber-reinforced alumina ceramics. Background Art
[0002] Alumina ceramic materials have excellent physical and chemical properties such as high strength, high hardness, high temperature resistance, corrosion resistance, and high insulation. Alumina ceramic raw materials are abundant and low in price, and they are widely used in many fields. However, the fatal shortcomings of alumina ceramics, such as high brittleness and poor toughness, seriously limit their wide application. In addition, alumina ceramics have a high thermal expansion coefficient and low thermal conductivity, which makes it easy to generate thermal stress when heated. When the temperature gradient is large, the thermal stress will exceed the strength limit of alumina ceramics, causing them to rupture. Therefore, improving the thermal shock resistance of alumina ceramics is also a current research hotspot. Summary of the invention
[0003] Purpose of the invention: In view of the above technical problems, the present invention proposes a method for preparing modified fiber-reinforced alumina ceramics.
[0004] The technical solutions adopted are as follows:
[0005] A method for preparing modified fiber-reinforced alumina ceramics:
[0006] Firstly, eucryptite-coated modified alumina fiber is prepared, and then the eucryptite-coated modified alumina fiber, alumina powder and a sintering aid are mixed and ball-milled, dried, granulated, pressed and sintered.
[0007] Furthermore, the sintering aid includes alkaline earth metal oxides, rare earth fluorides and YMO3, wherein M is any one of B, Ti, Fe and Al.
[0008] Furthermore, the weight ratio of the alkaline earth metal oxide, rare earth fluoride and YMO3 is 1-5:1-5:1-5.
[0009] Furthermore, the rare earth fluoride is lanthanum fluoride and / or cerium fluoride.
[0010] Further, M is B.
[0011] Furthermore, the weight ratio of the eucryptite-coated modified alumina fiber, alumina powder and sintering aid is 5-15:80-100:1-5.
[0012] Furthermore, the preparation method of the eucryptite-coated modified alumina fiber is as follows:
[0013] A water-soluble lithium salt and a water-soluble aluminum salt are dissolved in anhydrous ethanol to obtain a mixed solution, the hydrolyzate obtained by hydrolyzing tetraethyl orthosilicate is mixed with the mixed solution, and a citric acid ethanol solution and a dispersant are added. During the above process, the pH of the reaction system is always maintained at 3-4, and the reaction is heated in a water bath at 50-70°C for more than 30 minutes to obtain eucryptite gel. After the alumina fiber is immersed in the eucryptite gel, it is taken out and heat-treated at 900-1200°C in a tubular furnace for 1-3 hours.
[0014] Furthermore, the pressing pressure is ≥50 MPa.
[0015] Furthermore, during sintering, the temperature is first raised from room temperature to 100-150°C and kept for 1-10 hours, then raised to 500-650°C and kept for 1-4 hours, and finally raised to 1350-1500°C and kept for 2-4 hours.
[0016] Furthermore, the second stage heating rate is 10-30°C / min, and the third stage heating rate is 1-5°C / min.
[0017] Beneficial effects of the present invention:
[0018] The present invention provides a method for preparing modified fiber-reinforced alumina ceramics. The addition of alumina fibers can share the external load on the one hand, and absorb external energy through crack deflection or bifurcation, pull-out effect and bridging effect on the other hand, thereby achieving the purpose of improving the brittleness of alumina ceramics. The eucryptite coating modification significantly improves the bending strength and fracture toughness of alumina ceramics. The reason may be that the eucryptite coating layer can protect the alumina fibers from damage during the preparation process and the interface between the alumina matrix and the eucryptite can cause greater mechanical interlocking between phases, resulting in oxidation The aluminum fiber has longer debonding and bridging, which improves the bending strength and fracture toughness. Alkaline earth metal oxides and rare earth fluorides can produce liquid phases during the sintering process. The liquid phase fills the pores through its surface tension, which can inhibit the recrystallization of grains to a certain extent, promote the sintering process, and reduce the sintering temperature. The addition of YMO3 can promote particle rearrangement, make the grains more closely bonded, improve the ceramic density, improve the thermal conductivity, and improve the thermal shock resistance. The alumina ceramics prepared by the present invention have good mechanical properties, with a bending strength of ≥410MPa and a fracture toughness of ≥4.4MPa·m 1 / 2 , and has excellent high temperature thermal shock resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a microscopic morphology of the eucryptite-coated modified alumina fiber prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0020] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.
[0021] Embodiment 1:
[0022] A method for preparing modified fiber-reinforced alumina ceramics:
[0023] 6.89 g lithium nitrate and 21.3 g aluminum nitrate were dissolved in 75 ml anhydrous ethanol to obtain a mixed solution. 20.8 g ethyl orthosilicate was added to 125 ml anhydrous ethanol / water solution (pH 3-4) 无水乙醇 / V 水 =4:1) for 30 min to obtain a hydrolyzate, the hydrolyzate and the mixed solution are mixed, 100 ml of 2 mol / L citric acid ethanol solution and 10 g of dispersant polyethylene glycol 2000 are added dropwise, the pH of the reaction system is always kept at 3-4 during the above process, and the eucryptite gel is obtained by heating at 60°C in a water bath for 45 min. The alumina fiber is immersed in the eucryptite gel at room temperature for 10 min, then taken out and heat-treated at 1000°C in a tube furnace for 1 h to obtain the eucryptite-coated modified alumina fiber, and the eucryptite-coated modified Alumina fiber, alumina powder, magnesium oxide, lanthanum fluoride and yttrium borate are added to a planetary ball mill, ethanol is used as the ball milling medium, the mixture is ball-milled for 5 hours and then dried, 5wt% polyvinyl alcohol is added as a binder to granulate, and the green body is pressed at 100 MPa to obtain a green body. Finally, the green body is placed in a tubular furnace in an air atmosphere and heated from room temperature to 120°C at a rate of 20°C / min in one stage and kept warm for 5 hours, then heated to 600°C at a rate of 10°C / min in two stages and kept warm for 2 hours, finally heated to 1450°C at a rate of 2°C / min in three stages and kept warm for 3 hours, and finally the furnace is cooled to room temperature.
[0024] Embodiment 2:
[0025] A method for preparing modified fiber-reinforced alumina ceramics:
[0026] 6.89 g lithium nitrate and 21.3 g aluminum nitrate were dissolved in 75 ml anhydrous ethanol to obtain a mixed solution. 20.8 g ethyl orthosilicate was added to 125 ml anhydrous ethanol / water solution (pH 3-4) 无水乙醇 / V 水=4:1) for 30 min to obtain a hydrolyzate, the hydrolyzate and the mixed solution were mixed, 100 ml of 2 mol / L citric acid ethanol solution and 10 g of dispersant polyethylene glycol 2000 were added dropwise, the pH of the reaction system was always kept at 3-4 during the above process, and 60°C water bath was heated for 45 min to obtain eucryptite gel, the alumina fiber was immersed in the eucryptite gel at room temperature for 10 min, then taken out and heat treated at 1000°C in a tube furnace for 1 h to obtain eucryptite coated modified alumina fiber, the eucryptite coated modified alumina fiber with a weight ratio of 15:100:2:1:1 was prepared by dipping the alumina fiber in the eucryptite gel at room temperature for 10 min, then taking out the alumina fiber and heat treating it in a tube furnace at 1000°C for 1 h to obtain the eucryptite coated modified alumina fiber, Alumina fiber, alumina powder, magnesium oxide, lanthanum fluoride and yttrium borate are added to a planetary ball mill, ethanol is used as the ball milling medium, the mixture is ball-milled for 5 hours and then dried, 5wt% polyvinyl alcohol is added as a binder to granulate, and the green body is pressed at 100 MPa to obtain a green body, and finally the green body is placed in a tubular furnace in an air atmosphere, the temperature is increased from room temperature to 150°C at a rate of 20°C / min in one stage and kept warm for 5 hours, and then the temperature is increased to 650°C in two stages at a rate of 10°C / min and kept warm for 4 hours, and finally the temperature is increased to 1500°C in three stages at a rate of 2°C / min and kept warm for 2 hours, and finally the furnace is cooled to room temperature.
[0027] Embodiment 3:
[0028] A method for preparing modified fiber-reinforced alumina ceramics:
[0029] 6.89 g lithium nitrate and 21.3 g aluminum nitrate were dissolved in 75 ml anhydrous ethanol to obtain a mixed solution. 20.8 g ethyl orthosilicate was added to 125 ml anhydrous ethanol / water solution (pH 3-4) 无水乙醇 / V 水 =4:1) for 30 min to obtain a hydrolyzate, the hydrolyzate and the mixed solution are mixed, 100 ml of 2 mol / L citric acid ethanol solution and 10 g of dispersant polyethylene glycol 2000 are added dropwise, the pH of the reaction system is always kept at 3-4 during the above process, and the eucryptite gel is obtained by heating at 60°C in a water bath for 45 min, the alumina fiber is immersed in the eucryptite gel at room temperature for 10 min, then taken out and heat-treated at 1000°C in a tubular furnace for 1 h to obtain the eucryptite-coated modified alumina fiber, and the eucryptite-coated modified Alumina fiber, alumina powder, magnesium oxide, lanthanum fluoride and yttrium borate are added to a planetary ball mill, ethanol is used as the ball milling medium, the mixture is ball-milled for 5 hours and then dried, 5wt% polyvinyl alcohol is added as a binder for granulation, and the green body is pressed at 100 MPa to obtain a green body. Finally, the green body is placed in a tubular furnace in an air atmosphere and heated from room temperature to 100°C at a rate of 20°C / min in one stage and kept warm for 10 hours, then heated to 550°C in two stages at a rate of 10°C / min and kept warm for 2 hours, finally heated to 1350°C in three stages at a rate of 2°C / min and kept warm for 2 hours, and finally the furnace is cooled to room temperature.
[0030] Comparative Example 1:
[0031] It is basically the same as Example 1, except that the alumina fiber is added directly without being modified by coating with eucryptite.
[0032] Comparative Example 2:
[0033] The method is basically the same as Example 1, except that magnesium oxide is not added.
[0034] Comparative Example 3:
[0035] The method is substantially the same as Example 1, except that lanthanum fluoride is not added.
[0036] Comparative Example 4:
[0037] The method is substantially the same as Example 1, except that yttrium borate is not added.
[0038] Performance Test:
[0039] The alumina ceramics prepared in Examples 1-3 and Comparative Examples 1-4 were made into samples for performance testing;
[0040] The three-point bending method was used to test the specimens. The method was based on the standard GBT6569-2006. The equipment was an electronic universal testing machine (model WDW-100). The size of the specimen was 50 mm × 5 mm × 3 mm (length × width × height). During the test, the span was selected as 40 mm and the loading rate was selected as 0.5 mm / min.
[0041] The fracture toughness of the sample was tested by the single-sided notched beam method. The size of the sample was 40 mm × 3 mm × 6 mm (length × width × height), the prefabricated notch depth was 3 mm, the span was selected as 30 mm during the test, and the loading rate was selected as 0.05 mm / min.
[0042] The sample was heated to 1400°C at a rate of 10°C / min, kept warm for 30 minutes, and then quickly cooled to room temperature using a cold high-pressure air flow. The heating and cooling operations were repeated 10 times. The bending strength and fracture toughness of the sample were tested, and the decline rate was calculated to characterize the high-temperature thermal shock resistance of alumina ceramics.
[0043] The test results are shown in Table 1:
[0044] Table 1:
[0045]
[0046] It can be seen from Table 1 above that the alumina ceramics prepared by the present invention have good mechanical properties, with a bending strength of ≥410MPa and a fracture toughness of ≥4.4MPa·m 1 / 2 , and has excellent high temperature thermal shock resistance.
[0047] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing modified fiber-reinforced alumina ceramics, characterized in that: First, eucryptite-coated modified alumina fiber is prepared, and then the eucryptite-coated modified alumina fiber, alumina powder and a sintering aid are mixed and ball-milled, dried, granulated, pressed and sintered; During sintering, the temperature is first raised from room temperature to 100-150℃ and kept for 1-10h, then raised to 500-650℃ and kept for 1-4h, and finally raised to 1350-1500℃ and kept for 2-4h. The sintering aids include alkaline earth metal oxides, rare earth fluorides and YBO3; The weight ratio of the alkaline earth metal oxide, rare earth fluoride and YBO3 is 1-5:1-5:1-5; The weight ratio of the eucryptite-coated modified alumina fiber, alumina powder and sintering aid is 5-15:80-100:1-5; The preparation method of the eucryptite-coated modified alumina fiber is as follows: A water-soluble lithium salt and a water-soluble aluminum salt are dissolved in anhydrous ethanol to obtain a mixed solution, the hydrolyzate obtained by hydrolyzing tetraethyl orthosilicate is mixed with the mixed solution, and a citric acid ethanol solution and a dispersant are added. During the above process, the pH of the reaction system is always maintained at 3-4, and the reaction is heated in a water bath at 50-70°C for more than 30 minutes to obtain eucryptite gel. After the alumina fiber is immersed in the eucryptite gel, it is taken out and heat-treated at 900-1200°C in a tubular furnace for 1-3 hours.
2. The preparation method according to claim 1, characterized in that The rare earth fluoride is lanthanum fluoride and / or cerium fluoride.
3. The preparation method according to claim 1, characterized in that: The pressing pressure is ≥50MPa.
4. The preparation method according to claim 1, characterized in that: The second stage heating rate is 10-30°C / min, and the third stage heating rate is 1-5°C / min.
Citation Information
Patent Citations
Method for preparing microcrystalline glass composite material containing alumina
CN101565323A
Continuous alumina fiber reinforced aluminum-based composite material and preparation method thereof