A polytetrafluoroethylene material for spring sealing ring and its preparation method and application
Through pretreatment and multi-step modification treatment, nano yttrium oxide/graphene oxide filled foamed polytetrafluoroethylene material is formed, which solves the shortcomings of polytetrafluoroethylene sealing materials in antistatic, mechanical and frictional properties, and achieves more Good sealing effect and service life.
Patent Information
- Application Number
- CN202410635472.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-05-22
AI Technical Summary
The existing polytetrafluoroethylene sealing materials have shortcomings in antistatic, mechanical properties and friction and wear properties, and the filling materials have limited performance improvement effects and cannot take into account the overall performance.
By using pretreatment, foaming, cell filling, reduction and modification steps, polytetrafluoroethylene is mixed with naphthalene foaming agent, molding and soaking in yttrium nitrate and graphene oxide solutions, followed by reduction of hydrazine hydrate and Stearic acid lubricating oil treatment to form nano yttrium oxide/graphene oxide filled foamed polytetrafluoroethylene material.
It improves the anti-static, mechanical properties and wear-resistant lubrication properties of polytetrafluoroethylene materials, provides a long-term sealing effect, and protects the spring metal, extending service life.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sealing materials, and in particular to a polytetrafluoroethylene material for a spring sealing ring and a preparation method and application thereof. Background Art
[0002] The single-point mooring slip ring is a key equipment for connecting the floating production storage and offloading unit (FPSO) with the underwater production system. Its main function is to achieve continuous transportation of the medium when the floating body rotates. The energy storage spring seal is a key component of the single-point mooring slip ring. It is a self-tightening seal that achieves effective sealing through the increase in sealing contact pressure when the system pressure increases. Its quality directly affects the working performance of the slip ring. At present, the technical monopoly of single-point mooring slip rings and energy storage spring seals is very serious. The related products used in Chinese waters are all produced by foreign companies.
[0003] Polytetrafluoroethylene is a commonly used sealing material, but unfilled polytetrafluoroethylene has low load-bearing capacity, is prone to creep, is not wear-resistant, has a short life, and has a high resistivity. Filling polytetrafluoroethylene is the main way to improve the performance of polytetrafluoroethylene, such as filling polytetrafluoroethylene with metal powder (such as lead, nickel), solid lubricants (such as molybdenum disulfide) or other special nano-functional fillers (such as nano-alumina, nano-silicon dioxide, nano-zinc oxide), but due to the limitations and pertinence of a specific filler on the performance improvement of polytetrafluoroethylene, it is impossible to achieve an overall improvement in the comprehensive performance of polytetrafluoroethylene. The current filled polytetrafluoroethylene materials still find it difficult to balance antistatic properties, mechanical properties, and friction and wear properties.
[0004] Chinese patent document CN106928600A discloses a preparation method of a polytetrafluoroethylene coated rubber seal, wherein polytetrafluoroethylene is activated and modified by using sodium-naphthalene-tetrahydrofuran modified treatment liquid, and a mixture of styrene-butadiene rubber, acetylene black, acetate, 4-methyl-6-tert-butylphenol, 4,4'-thiobis(3-methyl-6-tert-butylphenol), vinyl tris(β-methoxyethoxy)silane is added to carry out modified roller refining, high temperature and high pressure reaction, mold base soaking and curing, high temperature and high pressure sintering, demoulding vulcanization, sintering and shaping, standing at room temperature, lathe processing and other series of operations to obtain a seal finished product. The prepared polytetrafluoroethylene coated rubber seal has high aging resistance, high toughness, low friction coefficient and good sealing performance, and has good application prospects. However, the method adopts simple mechanical mixing, and it is impossible to achieve sufficient uniform mixing, and there are problems such as poor dispersibility of modifiers, and the material properties that cannot be significantly improved. Summary of the invention
[0005] The purpose of the present invention is to provide a polytetrafluoroethylene material for a spring sealing ring and a preparation method and application thereof. The preparation method is simple, the raw material source is wide, the cost is low, the material has good wear resistance and lubrication, and the antistatic and mechanical properties of the polytetrafluoroethylene material are improved, so that the material can provide a long-term sealing effect and can also protect the spring metal, thereby increasing its service life and having broad application prospects.
[0006] The technical solution of the present invention is achieved in this way:
[0007] The present invention provides a method for preparing a polytetrafluoroethylene material for a spring sealing ring, comprising the following steps:
[0008] S1. Pretreatment: drying the polytetrafluoroethylene resin, mixing it with the foaming agent, and ball milling it, and sieving it to obtain a mixed powder;
[0009] S2. Preparation of polytetrafluoroethylene foam: adding the mixed powder in step S1 to a mold, compression molding, standing, sintering, to obtain polytetrafluoroethylene foam;
[0010] S3. Pore filling: dissolving yttrium nitrate and graphene oxide in water, adjusting the pH value of the solution, adding a mixed solution of urea and polyethylene glycol 2000 dropwise, soaking the foamed polytetrafluoroethylene obtained in step S2 in the solution, and after the liquid is completely absorbed, heating the reaction, aging, washing, drying, sintering, and filling the foamed polytetrafluoroethylene with nano-yttrium oxide / graphene oxide;
[0011] S4 reduction: the nano yttrium oxide / graphene oxide filled polytetrafluoroethylene foam obtained in step S3 is reduced by hydrazine hydrate vapor to obtain filled polytetrafluoroethylene foam;
[0012] S5. Modification: Dissolve stearic acid in lubricating oil, put the filled foamed polytetrafluoroethylene obtained in step S4 into the mixed solution, heat to react, cool to room temperature, take out, and obtain a polytetrafluoroethylene material for a spring seal ring.
[0013] As a further improvement of the present invention, the drying temperature in step S1 is 100-105° C., the time is 0.5-1.5 h, the ball milling time is 1-2 h, the sieving mesh size is 200-300 mesh, and the mass ratio of the polytetrafluoroethylene resin to the foaming agent is 100:8-12.
[0014] As a further improvement of the present invention, the foaming agent is naphthalene.
[0015] As a further improvement of the present invention, the compression molding pressure in step S2 is 35-45 MPa, the static time is 20-24 h, the sintering temperature is 350-380° C., and the time is 0.5-1.5 h.
[0016] As a further improvement of the present invention, the mass ratio of yttrium nitrate, graphene oxide, urea, polyethylene glycol 2000 and foamed polytetrafluoroethylene in step S3 is 7-10:2-4:0.2-0.4:0.5-1:100, the pH value of the adjusted solution is 8-9, the temperature of the heating reaction is 65-75°C, the time is 1-3h, the aging time is 0.5-1h, and the sintering temperature is 350-380°C, and the time is 0.5-1.5h.
[0017] As a further improvement of the present invention, the reduction time in step S4 is 10-12 hours.
[0018] As a further improvement of the present invention, in step S5, the mass ratio of stearic acid, lubricating oil and filled foamed polytetrafluoroethylene is 3-5:60-70:100, the temperature of the heating reaction is 90-95° C., and the time is 12-15 hours.
[0019] As a further improvement of the present invention, the present invention specifically comprises the following steps:
[0020] S1 pretreatment: 100 parts by weight of polytetrafluoroethylene resin 100-105 ℃ dried 0.5-1.5h, mixed with 8-12 parts by weight of blowing agent naphthalene ball milled 1-2h, through a 200-300 mesh sieve to obtain a mixed powder;
[0021] S2. Preparation of foamed polytetrafluoroethylene: The mixed powder in step S1 is added to a mold, compression molded at a pressure of 35-45MPa, allowed to stand for 20-24h, sintered at 350-380°C for 0.5-1.5h to obtain foamed polytetrafluoroethylene;
[0022] S3. Cell filling: 7-10 parts by weight of yttrium nitrate and 2-4 parts by weight of graphene oxide are dissolved in 100 parts by weight of water, the pH value of the solution is adjusted to 8-9, 10 parts by weight of an aqueous solution containing 0.2-0.4 parts by weight of urea and 0.5-1 parts by weight of polyethylene glycol 2000 are added dropwise, 100 parts by weight of the foamed polytetrafluoroethylene prepared in step S2 are immersed in the solution, and after the liquid is completely absorbed, heated to 65-75 ° C, reacted for 1-3h, aged for 0.5-1h, washed, dried, sintered at 350-380 ° C for 0.5-1.5h, and the nano-yttrium oxide / graphene oxide is filled with foamed polytetrafluoroethylene;
[0023] S4 reduction: the nano yttrium oxide / graphene oxide filled polytetrafluoroethylene foam obtained in step S3 was reduced by hydrazine hydrate vapor for 10-12h to obtain filled polytetrafluoroethylene foam;
[0024] S5. Modification: Dissolve 3-5 parts by weight of stearic acid in 60-70 parts by weight of lubricating oil, put 100 parts by weight of the filled foamed polytetrafluoroethylene obtained in step S4 into the mixed solution, and after the liquid is completely absorbed, heat to 90-95°C, react for 12-15 hours, cool to room temperature, take out, and obtain a polytetrafluoroethylene material for a spring sealing ring.
[0025] The present invention further protects a polytetrafluoroethylene material for a spring sealing ring obtained by the above-mentioned preparation method.
[0026] The present invention further protects the use of the polytetrafluoroethylene material for the spring seal ring in the preparation of a single-point mooring liquid slip ring.
[0027] The present invention has the following beneficial effects:
[0028] The foamed modified polytetrafluoroethylene sealing material has better elasticity, flexibility and creep relaxation resistance, and better long-term sealing effect. The present invention infiltrates solid foaming agent naphthalene into PTFE resin powder to make a rough finished product, allowing the foaming agent to occupy a certain space in the polytetrafluoroethylene material product, and then removes the foaming agent by a physical sintering method, so that the space originally occupied by the foaming agent becomes micropores, and foamed polytetrafluoroethylene is obtained.
[0029] Yttrium oxide has a unique 4f electronic layer structure, has obvious anti-wear and friction-reducing effect, and has excellent anti-wear and lubrication performance. However, due to its small particle size, large specific surface area, high surface activity, and easy agglomeration, it is difficult to be widely used. If it is directly added to the non-polar system polytetrafluoroethylene, the surface performance of nano yttrium oxide is polarity, and it cannot be stably dispersed, and its superior performance cannot be brought into play. Therefore, the present invention is by immersing foamed polytetrafluoroethylene in a solution containing yttrium nitrate and graphene oxide, and the foamed polytetrafluoroethylene fully absorbs liquid, and by adding a precipitant, a composite of yttrium oxide and graphene oxide is formed in situ in the pores, so that yttrium oxide is fully dispersed, thereby giving play to good wear-resistant, lubricating and other properties. Further, graphene is obtained through hydrazine hydrate reduction to have good electrical conductivity, greatly improving the electrical conductivity and antistatic properties of the obtained polytetrafluoroethylene material, and due to uniform dispersion, its mechanical properties are also significantly improved.
[0030] Stearic acid is green, environmentally friendly and low-priced. As a long-chain fatty acid, it further reacts with the modifier in the pores to further improve the anti-wear, friction reduction and lubrication effects of the polytetrafluoroethylene material. At the same time, the foamed polytetrafluoroethylene also fully absorbs the lubricating oil. Due to its internal porous structure, it can absorb and store the lubricating oil. When the temperature and pressure change during work, the lubricating oil seeps out through capillary action to form a lubricating film and play a lubricating role. When the working pressure and temperature return to the initial state, part of the lubricating oil can be absorbed into the pores of the material through capillary action, thereby achieving good self-lubrication and providing a longer-lasting sealing effect. At the same time, the stearic acid, lubricating oil and graphene therein can also protect the spring metal and increase its service life.
[0031] The polytetrafluoroethylene material for the spring sealing ring prepared by the present invention has a simple preparation method, a wide source of raw materials, low cost, good wear resistance and lubrication, and improves the antistatic and mechanical properties of the polytetrafluoroethylene material, so that it can provide a long-term sealing effect and protect the spring metal, thereby increasing its service life and having broad application prospects. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Polytetrafluoroethylene resin, M18F, was purchased from Daikin Co., Ltd., Japan.
[0034] Graphene oxide was purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.
[0035] Lubricating oil, density 0.8-0.82g / cm 3 , flash point 110-150℃, purchased from Shandong Taichang Petrochemical Technology Co., Ltd.
[0036] Example 1
[0037] This embodiment provides a method for preparing a polytetrafluoroethylene material for a spring sealing ring, comprising the following steps:
[0038] S1. Pretreatment: 100 g of polytetrafluoroethylene resin was dried at 100 ° C for 0.5 h, mixed with 8 g of naphthalene foaming agent and ball-milled for 1 h, and passed through a 200-mesh sieve to obtain a mixed powder;
[0039] S2. Preparation of polytetrafluoroethylene foam: The mixed powder in step S1 was added to a mold, compression molded at a pressure of 35 MPa, allowed to stand for 20 h, and sintered at 350 ° C for 0.5 h to obtain polytetrafluoroethylene foam;
[0040] S3. Cell filling: 7 g of yttrium nitrate and 2 g of graphene oxide were dissolved in 100 g of water, the pH value of the solution was adjusted to 8, 10 g of an aqueous solution containing 0.2 g of urea and 0.5 g of polyethylene glycol 2000 was added dropwise, 100 g of the foamed polytetrafluoroethylene prepared in step S2 was immersed in the solution, and after the liquid was completely absorbed, it was heated to 65 ° C, reacted for 1 h, aged for 0.5 h, washed, dried, and sintered at 350 ° C for 0.5 h to obtain nano yttrium oxide / graphene oxide filled foamed polytetrafluoroethylene;
[0041] S4 reduction: the nano yttrium oxide / graphene oxide filled polytetrafluoroethylene foam obtained in step S3 was reduced by hydrazine hydrate vapor for 10h to obtain filled polytetrafluoroethylene foam;
[0042] S5. Modification: Dissolve 3g of stearic acid in 60g of lubricating oil, put 100g of the filled foamed polytetrafluoroethylene obtained in step S4 into the mixed liquid, and after the liquid is completely absorbed, heat to 90°C, react for 12h, cool to room temperature, take out, and obtain a polytetrafluoroethylene material for a spring sealing ring.
[0043] Example 2
[0044] This embodiment provides a method for preparing a polytetrafluoroethylene material for a spring sealing ring, comprising the following steps:
[0045] S1. Pretreatment: 100 g of polytetrafluoroethylene resin was dried at 105 ° C for 1.5 h, mixed with 12 g of naphthalene foaming agent and ball-milled for 2 h, and passed through a 300-mesh sieve to obtain a mixed powder;
[0046] S2. Preparation of foamed polytetrafluoroethylene: The mixed powder in step S1 was added to a mold, compression molded at a pressure of 45 MPa, allowed to stand for 24 h, and sintered at 380 ° C for 1.5 h to obtain foamed polytetrafluoroethylene;
[0047] S3. Cell filling: 10 g of yttrium nitrate and 4 g of graphene oxide were dissolved in 100 g of water, the pH value of the solution was adjusted to 9, 10 g of an aqueous solution containing 0.4 g of urea and 1 g of polyethylene glycol 2000 was added dropwise, 100 g of the foamed polytetrafluoroethylene prepared in step S2 was immersed in the solution, and after the liquid was completely absorbed, it was heated to 75 ° C, reacted for 3 h, aged for 1 h, washed, dried, and sintered at 380 ° C for 1.5 h to obtain nano yttrium oxide / graphene oxide filled foamed polytetrafluoroethylene;
[0048] S4 reduction: the nano yttrium oxide / graphene oxide filled polytetrafluoroethylene foam obtained in step S3 was reduced by hydrazine hydrate vapor for 12h to obtain filled polytetrafluoroethylene foam;
[0049] S5. Modification: Dissolve 5 g of stearic acid in 70 g of lubricating oil, put 100 g of the filled foamed polytetrafluoroethylene obtained in step S4 into the mixture, and after the liquid is completely absorbed, heat to 95°C, react for 15 hours, cool to room temperature, take out, and obtain a polytetrafluoroethylene material for a spring sealing ring.
[0050] Example 3
[0051] This embodiment provides a method for preparing a polytetrafluoroethylene material for a spring sealing ring, comprising the following steps:
[0052] S1. Pretreatment: 100 g of polytetrafluoroethylene resin was dried at 105 ° C for 1 h, mixed with 10 g of naphthalene foaming agent and ball-milled for 1.5 h, and passed through a 300-mesh sieve to obtain a mixed powder;
[0053] S2. Preparation of foamed polytetrafluoroethylene: The mixed powder in step S1 was added to a mold, compression molded at a pressure of 40 MPa, allowed to stand for 22 h, and sintered at 365 ° C for 1 h to obtain foamed polytetrafluoroethylene;
[0054] S3. Cell filling: 8.5 g of yttrium nitrate and 3 g of graphene oxide were dissolved in 100 g of water, the pH value of the solution was adjusted to 8.5, 10 g of an aqueous solution containing 0.3 g of urea and 0.7 g of polyethylene glycol 2000 was added dropwise, 100 g of the foamed polytetrafluoroethylene prepared in step S2 was immersed in the solution, and after the liquid was completely absorbed, it was heated to 70 ° C, reacted for 2 h, aged for 1 h, washed, dried, and sintered at 365 ° C for 1 h to obtain nano-yttrium oxide / graphene oxide filled foamed polytetrafluoroethylene;
[0055] S4 reduction: the nano yttrium oxide / graphene oxide filled polytetrafluoroethylene foam obtained in step S3 was reduced by hydrazine hydrate vapor for 11h to obtain filled polytetrafluoroethylene foam;
[0056] S5. Modification: Dissolve 4 g of stearic acid in 65 g of lubricating oil, put 100 g of the filled foamed polytetrafluoroethylene obtained in step S4 into the mixture, and after the liquid is completely absorbed, heat to 92°C, react for 13 hours, cool to room temperature, take out, and obtain a polytetrafluoroethylene material for a spring sealing ring.
[0057] Comparative Example 1
[0058] Compared with Example 3, the difference is that graphene oxide is not added in step S3.
[0059] The details are as follows:
[0060] S3. Pore filling: 11.5 g of yttrium nitrate was dissolved in 100 g of water, the pH value of the solution was adjusted to 8.5, 10 g of an aqueous solution containing 0.3 g of urea and 0.7 g of polyethylene glycol 2000 was added dropwise, 100 g of the foamed polytetrafluoroethylene obtained in step S2 was immersed in the solution, and after the liquid was completely absorbed, it was heated to 70°C, reacted for 2 h, aged for 1 h, washed, dried, and sintered at 365°C for 1 h to obtain nano yttrium oxide / graphene oxide filled foamed polytetrafluoroethylene.
[0061] Comparative Example 2
[0062] Compared with Example 3, the difference is that yttrium nitrate is not added in step S3.
[0063] The details are as follows:
[0064] S3. Pore filling: add 11.5 g of graphene oxide to 100 g of water, adjust the pH value of the solution to 8.5, add dropwise 10 g of an aqueous solution containing 0.3 g of urea and 0.7 g of polyethylene glycol 2000, immerse 100 g of foamed polytetrafluoroethylene obtained in step S2 in the solution, and after the liquid is completely absorbed, heat to 70°C, react for 2 h, age for 1 h, wash, dry, and sinter at 365°C for 1 h to obtain graphene oxide-filled foamed polytetrafluoroethylene.
[0065] Comparative Example 3
[0066] Compared with Example 3, the difference is that step S4 is not performed.
[0067] The details are as follows:
[0068] S1. Pretreatment: The polytetrafluoroethylene resin was dried at 105°C for 1h, mixed with the blowing agent naphthalene and ball-milled for 1.5h, and passed through a 300-mesh sieve to obtain a mixed powder;
[0069] S2. Preparation of foamed polytetrafluoroethylene: The mixed powder in step S1 was added to a mold, compression molded at a pressure of 40 MPa, allowed to stand for 22 h, and sintered at 365 ° C for 1 h to obtain foamed polytetrafluoroethylene;
[0070] S3. Cell filling: 8.5 g of yttrium nitrate and 3 g of graphene oxide were dissolved in 100 g of water, the pH value of the solution was adjusted to 8.5, 10 g of an aqueous solution containing 0.3 g of urea and 0.7 g of polyethylene glycol 2000 was added dropwise, 100 g of the foamed polytetrafluoroethylene prepared in step S2 was immersed in the solution, and after the liquid was completely absorbed, it was heated to 70 ° C, reacted for 2 h, aged for 1 h, washed, dried, and sintered at 365 ° C for 1 h to obtain nano-yttrium oxide / graphene oxide filled foamed polytetrafluoroethylene;
[0071] S4. Modification: Dissolve 4 g of stearic acid in 65 g of lubricating oil, put 100 g of nano-yttrium oxide / graphene oxide filled foamed polytetrafluoroethylene obtained in step S3 into the mixture, and after the liquid is completely absorbed, heat to 92°C, react for 13 hours, cool to room temperature, take out, and obtain a polytetrafluoroethylene material for a spring sealing ring.
[0072] Comparative Example 4
[0073] Compared with Example 3, the difference is that stearic acid is not added in step S5.
[0074] The details are as follows:
[0075] S5. Modification: Put 100 g of the filled foamed polytetrafluoroethylene obtained in step S4 into 69 g of lubricating oil. After the liquid is completely absorbed, heat to 92°C, react for 13 hours, cool to room temperature, take out, and obtain a polytetrafluoroethylene material for a spring sealing ring.
[0076] Comparative Example 5
[0077] Compared with Example 3, the difference is that steps S3 and S4 are not performed.
[0078] The details are as follows:
[0079] S1. Pretreatment: The polytetrafluoroethylene resin was dried at 105°C for 1h, mixed with the blowing agent naphthalene and ball-milled for 1.5h, and passed through a 300-mesh sieve to obtain a mixed powder;
[0080] S2. Preparation of foamed polytetrafluoroethylene: The mixed powder in step S1 was added to a mold, compression molded at a pressure of 40 MPa, allowed to stand for 22 h, and sintered at 365 ° C for 1 h to obtain foamed polytetrafluoroethylene;
[0081] S3. Modification: Dissolve 4 g of stearic acid in 65 g of lubricating oil, put 100 g of foamed polytetrafluoroethylene obtained in step S2 into the mixture, and after the liquid is completely absorbed, heat to 92°C, react for 13 hours, cool to room temperature, take out, and obtain polytetrafluoroethylene material for spring sealing ring.
[0082] Test Example 1
[0083] The polytetrafluoroethylene materials used for the spring seal rings prepared in Examples 1-3 of the present invention and Comparative Examples 1-5 were subjected to mechanical property tests.
[0084] The elongation at break and tensile strength refer to the standard test method of GB / T1040-2018.
[0085] The elastic index test adopts the standard experimental method of ASTM F36, the sample size is 12mm×10mm, the experimental load is 245N, and the experimental temperature is 23±2℃.
[0086] The results are shown in Table 1.
[0087] Table 1
[0088] Group Elongation at break (%) Tensile strength(MPa) elasticity(%) Example 1 457 44.2 15.24 Example 2 455 43.9 15.17 Example 3 462 44.7 15.75 Comparative Example 1 424 40.1 13.27 Comparative Example 2 434 41.2 11.74 Comparative Example 3 440 42.4 13.92 Comparative Example 4 445 43.1 14.07 Comparative Example 5 345 22.9 10.04
[0089] It can be seen from the above table that the polytetrafluoroethylene material used for the spring sealing rings prepared in Examples 1-3 of the present invention has good mechanical properties and high elasticity.
[0090] Test Example 2
[0091] The polytetrafluoroethylene materials used for the spring seal rings prepared in Examples 1-3 of the present invention and Comparative Examples 1-5 were subjected to a wear resistance test.
[0092] Friction coefficient and volume wear rate: refer to GB / T3960-2016 test, 200N, 0.43m / s, the friction pair is GCr15 bearing steel, the wear sample size is 30mm×7mm×4mm, dry friction, and the friction time is 60min.
[0093] The results are shown in Table 2.
[0094] Table 2
[0095] Group Friction coefficient <![CDATA[Volume wear rate (mm 3 / N·m)]]> Example 1 0.11 <![CDATA[2.2×10 -7 ]]> Example 2 0.10 <![CDATA[1.9×10 -7 ]]> Example 3 0.10 <![CDATA[1.7×10 -7 ]]> Comparative Example 1 0.15 <![CDATA[3.1×10 -6 ]]> Comparative Example 2 0.25 <![CDATA[7.0×10 -6 ]]> Comparative Example 3 0.21 <![CDATA[5.7×10 -6 ]]> Comparative Example 4 0.17 <![CDATA[4.4×10 -6 ]]> Comparative Example 5 0.28 <![CDATA[7.6×10 -6 ]]>
[0096] It can be seen from the above table that the polytetrafluoroethylene material used for the spring sealing rings prepared in Examples 1-3 of the present invention has a small friction coefficient and has good wear resistance.
[0097] Test Example 3
[0098] The surface resistance of the polytetrafluoroethylene materials used for the spring seal rings prepared in Examples 1-3 of the present invention and Comparative Examples 1-5 was tested.
[0099] The results are shown in Table 3.
[0100] Table 3
[0101] Group Surface resistance(Ω) Example 1 <![CDATA[2.2×10 6 ]]> Example 2 <![CDATA[1.8×10 6 ]]> Example 3 <![CDATA[1.7×10 6 ]]> Comparative Example 1 <![CDATA[9.2×10 8 ]]> Comparative Example 2 <![CDATA[7.5×10 7 ]]> Comparative Example 3 <![CDATA[1.2×10 9 ]]> Comparative Example 4 <![CDATA[4.1×10 6 ]]> Comparative Example 5 <![CDATA[8.4×10 9 ]]>
[0102] It can be seen from the above table that the polytetrafluoroethylene material used for the spring sealing rings prepared in Examples 1-3 of the present invention has improved conductivity and better antistatic performance.
[0103] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a polytetrafluoroethylene material for a spring seal ring, characterized in that: The following steps are involved: S1. Pretreatment: drying the polytetrafluoroethylene resin, mixing it with the foaming agent, and ball milling it, and sieving it to obtain a mixed powder; S2. Preparation of polytetrafluoroethylene foam: adding the mixed powder in step S1 to a mold, compression molding, standing, sintering, to obtain polytetrafluoroethylene foam; S3. Pore filling: dissolving yttrium nitrate and graphene oxide in water, adjusting the pH value of the solution, adding a mixed solution of urea and polyethylene glycol 2000 dropwise, soaking the foamed polytetrafluoroethylene obtained in step S2 in the solution, and after the liquid is completely absorbed, heating the reaction, aging, washing, drying, sintering, and filling the foamed polytetrafluoroethylene with nano-yttrium oxide / graphene oxide; S4 reduction: the nano yttrium oxide / graphene oxide filled polytetrafluoroethylene foam obtained in step S3 is reduced by hydrazine hydrate vapor to obtain filled polytetrafluoroethylene foam; S5. Modification: Dissolve stearic acid in lubricating oil, put the filled foamed polytetrafluoroethylene obtained in step S4 into the mixed solution, heat to react, cool to room temperature, take out, and obtain a polytetrafluoroethylene material for a spring seal ring.
2. The preparation method according to claim 1, characterized in that: The drying temperature in step S1 is 100-105° C., the drying time is 0.5-1.5 h, the ball milling time is 1-2 h, the sieving mesh size is 200-300 mesh, and the mass ratio of the polytetrafluoroethylene resin to the foaming agent is 100:8-12.
3. The preparation method according to claim 1, characterized in that: The foaming agent is naphthalene.
4. The preparation method according to claim 1, characterized in that: The compression molding pressure in step S2 is 35-45 MPa, the static time is 20-24 h, the sintering temperature is 350-380° C., and the sintering time is 0.5-1.5 h.
5. The preparation method according to claim 1, characterized in that: The mass ratio of yttrium nitrate, graphene oxide, urea, polyethylene glycol 2000 and foamed polytetrafluoroethylene in step S3 is 7-10:2-4:0.2-0.4:0.5-1:100, the pH value of the adjusted solution is 8-9, the temperature of the heating reaction is 65-75°C, the time is 1-3h, the aging time is 0.5-1h, and the sintering temperature is 350-380°C, and the time is 0.5-1.5h.
6. The preparation method according to claim 1, characterized in that: The reduction time in step S4 is 10-12 hours.
7. The preparation method according to claim 1, characterized in that: In step S5, the mass ratio of stearic acid, lubricating oil and filled foamed polytetrafluoroethylene is 3-5:60-70:100, the temperature of the heating reaction is 90-95° C., and the time is 12-15 hours.
8. The preparation method according to claim 1, characterized in that: The specific steps include: S1 pretreatment: 100 parts by weight of polytetrafluoroethylene resin 100-105 ℃ dried 0.5-1.5h, mixed with 8-12 parts by weight of blowing agent naphthalene ball milled 1-2h, through a 200-300 mesh sieve to obtain a mixed powder; S2. Preparation of foamed polytetrafluoroethylene: The mixed powder in step S1 is added to a mold, compression molded at a pressure of 35-45MPa, allowed to stand for 20-24h, sintered at 350-380°C for 0.5-1.5h to obtain foamed polytetrafluoroethylene; S3. Cell filling: 7-10 parts by weight of yttrium nitrate and 2-4 parts by weight of graphene oxide are dissolved in 100 parts by weight of water, the pH value of the solution is adjusted to 8-9, 10 parts by weight of an aqueous solution containing 0.2-0.4 parts by weight of urea and 0.5-1 parts by weight of polyethylene glycol 2000 are added dropwise, 100 parts by weight of the foamed polytetrafluoroethylene prepared in step S2 are immersed in the solution, and after the liquid is completely absorbed, heated to 65-75 ° C, reacted for 1-3h, aged for 0.5-1h, washed, dried, sintered at 350-380 ° C for 0.5-1.5h, and the nano-yttrium oxide / graphene oxide is filled with foamed polytetrafluoroethylene; S4 reduction: the nano yttrium oxide / graphene oxide filled polytetrafluoroethylene foam obtained in step S3 was reduced by hydrazine hydrate vapor for 10-12h to obtain filled polytetrafluoroethylene foam; S5. Modification: Dissolve 3-5 parts by weight of stearic acid in 60-70 parts by weight of lubricating oil, put 100 parts by weight of the filled foamed polytetrafluoroethylene obtained in step S4 into the mixed solution, and after the liquid is completely absorbed, heat to 90-95°C, react for 12-15 hours, cool to room temperature, take out, and obtain a polytetrafluoroethylene material for a spring sealing ring.
9. A polytetrafluoroethylene material for a spring sealing ring obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the polytetrafluoroethylene material for the spring seal ring as claimed in claim 9 in the preparation of a single point mooring liquid slip ring.
Citation Information
Patent Citations
Preparation method of polytetrafluoroethylene coated rubber sealing part
CN106928600A
Preparation method of shock-absorbing noise-reducing rubber nano-composite material device
CN107522960A
Polytetrafluoroethylene high-frequency copper-clad plate with high thermal conductivity
CN111993720A
Antistatic polytetrafluoroethylene sealing material and preparation method thereof
CN114907656A
Mixed polytetrafluoroethylene powder, polytetrafluoroethylene porous shaped body, methods for producing those, polytetrafluoroethylene porous foam shaped body, and product for high-frequency signal transmission
US20070009727A1