A polycarbonate alloy and its preparation method and application

By combining modified sepiolite and potassium biphenyl sulfone-3 sulfonate, the problems of insufficient chemical solvent resistance, wear resistance and flame retardancy of polycarbonate alloys were solved, and alloy materials with excellent properties were prepared.

CN118496650BActive Publication Date: 2024-11-15GUANGDONG SEONLON NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410717859.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-11-15
Estimated Expiration
2044-06-04

AI Technical Summary

Technical Problem

Existing polycarbonate alloys have poor resistance to chemical solvents, wear resistance, and flame retardancy, which limits their application in many fields.

Method used

After pretreatment with materials such as sepiolite, PC, TPU, SBS, PETG and potassium biphenyl sulfone-3 sulfonate, the material is melt-extruded and granulated using a twin-screw extruder. γ-aminopropyltriethoxysilane is added to modify the sepiolite to improve compatibility, and combined with the flame-retardant effects of potassium biphenyl sulfone-3 sulfonate and RDP, a char layer is formed to enhance flame-retardant performance.

Benefits of technology

The resulting alloy material exhibits excellent chemical solvent resistance, wear resistance, and flame retardancy, significantly improving the overall performance of the polycarbonate alloy.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a polycarbonate alloy and a preparation method and application thereof, belonging to the technical field of alloys, and the preparation method of the polycarbonate alloy comprises the following steps: S1, pre-treating sepiolite, PC, TPU, SBS, PETG and potassium diphenyl sulfone-3 sulfonate respectively; S2, mixing functional additives, RDP and pre-treated sepiolite, PC, TPU, SBS, PETG, potassium diphenyl sulfone-3 sulfonate uniformly, placing in a twin-screw extruder melt extrusion granulation, temperature-controlled drying of the particles obtained by extrusion granulation and temperature-controlled injection molding into strips by an injection molding machine, i.e., finished alloy material. The finished alloy material obtained by the present invention has outstanding chemical solvent resistance, wear resistance and flame retardancy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of alloys, and in particular, relates to a polycarbonate alloy and a preparation method and application thereof. Background Art

[0002] Polycarbonate (PC) is a linear, almost colorless, glassy amorphous polymer with good impact strength, excellent electrical insulation, wide operating temperature range and good product dimensional stability. However, PC molecules contain a large number of benzene rings, and the molecular rigidity and steric hindrance are relatively large, so the flowability is poor during processing, the product is prone to stress cracking, and the residual stress is relatively large. In addition, there are problems such as low chemical solvent resistance, poor wear resistance, low surface hardness, and scratches after being scratched by hard objects, which limit its application in many fields. Therefore, PC is often melt-blended with other resins in industry to obtain alloys in order to improve its molding properties. There are many manufacturers on the market that use this melt-blending method to prepare alloy materials, but the chemical solvent resistance, wear resistance and flame retardant properties of the prepared alloy materials are not particularly excellent. Therefore, it is of great practical significance to provide a method for preparing a polycarbonate alloy to solve the above problems. Summary of the invention

[0003] The object of the present invention is to provide a polycarbonate alloy and a preparation method and application thereof, so as to solve the problem that the polycarbonate alloy in the prior art has poor chemical solvent resistance, wear resistance and flame retardancy.

[0004] The purpose of the present invention can be achieved by the following technical solutions:

[0005] A method for preparing a polycarbonate alloy, the preparation method specifically comprising the following steps:

[0006] S1, pre-treating sepiolite, PC, TPU, SBS, PETG and potassium diphenyl sulfone-3 sulfonate respectively;

[0007] S2. The functional additives, RDP and pretreated sepiolite, PC, TPU, SBS, PETG and potassium diphenyl sulfone-3 sulfonate are uniformly mixed, and the mixture is placed in a twin-screw extruder for melt extrusion granulation. The granules obtained by extrusion granulation are temperature-controlled dried and temperature-controlled injection-molded into strips by an injection molding machine to obtain a finished alloy material.

[0008] As a preferred technical solution of the present invention, the step S1 is specifically: ultrasonically dispersing sepiolite, deionized water and anhydrous ethanol to obtain a mixed solution A, controlling the temperature to adjust the pH of the mixed solution A to obtain a mixed solution B, adding γ-aminopropyltriethoxysilane to the mixed solution B, controlling the temperature and stirring, filtering, washing the filter residue, controlling the temperature to dry, grinding, and sieving to obtain the modified sepiolite for later use; controlling the temperature to dry PC, TPU, SBS, PETG and potassium diphenyl sulfone-3 sulfonate for later use.

[0009] The present invention adopts γ-aminopropyltriethoxysilane to modify sepiolite, thereby improving the compatibility of sepiolite with a base material, making it more evenly dispersed in the base material, and laying a foundation for preparing a finished alloy material with excellent flame retardant effect.

[0010] Furthermore, the usage ratio of the sepiolite, deionized water and anhydrous ethanol is 50-52 g:100-105 mL:400-410 mL; the mass ratio of the mixed solution B and γ-aminopropyltriethoxysilane is 1:0.1-0.12.

[0011] Furthermore, the particle size of the sepiolite is 10-30 μm.

[0012] Furthermore, the temperature control is used to adjust the pH of the mixed solution A to 55-60°C using a 1 mol / L hydrochloric acid solution; the temperature of the temperature control stirring is 60-65°C, and the time is 5-6h; the filter residue washing is performed by washing the filter residue with deionized water and anhydrous ethanol until the pH is neutral; the temperature of the temperature control drying is 75-80°C; and the screening is performed through a 250-270 mesh sieve.

[0013] As a preferred technical solution of the present invention, in step S1, the temperature of PC temperature-controlled drying is 115-120°C, the temperature of TPU temperature-controlled drying is 75-80°C, the temperature of SBS temperature-controlled drying is 70-80°C, the temperature of PETG temperature-controlled drying is 100-105°C, and the temperature of potassium diphenyl sulfone-3 sulfonate temperature-controlled drying is 110-120°C; the drying time of PC, TPU, SBS, PETG and potassium diphenyl sulfone-3 sulfonate is 2-3h.

[0014] As a preferred technical solution of the present invention, the mass ratio of the functional additive, RDP, pretreated sepiolite, pretreated PC, pretreated TPU, pretreated SBS, pretreated PETG, and pretreated potassium diphenyl sulfone-3 sulfonate in step S2 is 1-2.5:5-6:10-12:75-85:12-15:3.8-4.2:20-25:0.002-0.004.

[0015] As a preferred technical solution of the present invention, the extrusion temperature of each section of the extrusion granulation in step S2 is 200-220°C, and the screw speed is 200-220r / min.

[0016] As a preferred technical solution of the present invention, the temperature of the temperature-controlled drying in step S2 is 80-100°C and the time is 4-5h; the temperature of the temperature-controlled injection molding into the strip is 230-270°C.

[0017] As a preferred technical solution of the present invention, the PC grade in step S2 is PC-1201-10P, purchased from LG Polycarbonate Co., Ltd.; the TPU is a polyether TPU with a grade of WHT-8190, purchased from Wanhua Chemical Group Co., Ltd.; the SBS grade is Kraton D1116AIM, purchased from Shenzhen Yingqun Chemical Co., Ltd.; the functional additive is a functional additive of EVONIK brand with a grade of H-Si6441P, which is a granular polyester grafted modified silicone additive with good compatibility with plastic resin, purchased from Guangzhou Fantai New Material Technology Co., Ltd.; the PETG grade is K2012, purchased from SK Group of South Korea; the potassium diphenyl sulfone-3 sulfonate grade is KSS-FR103, purchased from Guangzhou Shanshan New Material Technology Co., Ltd.; the RDP is resorcinol bis(diphenyl phosphate), purchased from Shouguang Derun Chemical Co., Ltd.

[0018] The present invention also provides a polycarbonate alloy prepared by the method for preparing the polycarbonate alloy.

[0019] Furthermore, the present invention provides the use of the polycarbonate alloy in the manufacture of automobile parts, electronic and electrical products, office equipment products, packaging materials, building materials, etc.

[0020] Beneficial effects of the present invention:

[0021] (1) The present invention uses PC as the main base material to provide better toughness, but it still has the disadvantages of poor fluidity, poor wear resistance, and poor chemical resistance; therefore, on this basis, the present invention breaks through the use of TPU, SBS, H-SI6441P and PETG as the base material of the blended alloy material, making full use of the strengths of the performance of the four different raw materials, complementing each other's strengths, and synergizing to make the prepared alloy material have excellent solvent resistance and wear resistance. At present, in this field, no other companies have been found on the market to use base material composition formulas similar to the present invention to prepare alloy material products. Specifically, TPU is used to improve the processing fluidity of the blending system, reduce the internal stress, and thus improve the chemical solvent resistance of the finished alloy material; HSI 6441P, which has good self-lubrication and can reduce the surface scratch friction coefficient, is used to improve the surface scratch resistance of the finished alloy material; the polystyrene segment in SBS and the PC segment in the system are similarly compatible, so the physical volume expansion effect between PC and other base materials is increased; the excellent solvent resistance and wear resistance of PETG are used to further enhance the scratch resistance and chemical resistance of the finished alloy material; the finished alloy material thus obtained has outstanding chemical solvent resistance and wear resistance.

[0022] (2) The present invention adds potassium diphenyl sulfone-3 sulfonate to increase the carbonization rate of the system at high temperature and form a carbon layer on the surface of the finished alloy material, releasing non-combustibles, thereby blocking the air; the addition of RDP generates active free radicals containing phosphorus when subjected to high temperature, thereby preventing the combustion chain reaction from proceeding; on this basis, the sepiolite, whose crystal structure is formed by continuous silicon-oxygen tetrahedrons and discontinuous magnesium-oxygen octahedrons alternately connected with each other, further increases the density of the carbon layer formed by the system, thereby assisting potassium diphenyl sulfone-3 sulfonate and RDP to strengthen the system's ability to block heat and air, thereby enhancing the flame retardant properties of the finished alloy material. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Example 1

[0025] A method for preparing a polycarbonate alloy, the preparation method specifically comprising the following steps:

[0026] S1. Pre-treating sepiolite, PC, TPU, SBS, PETG and potassium diphenyl sulfone-3 sulfonate respectively, specifically:

[0027] Ultrasonic dispersion of sepiolite with a particle size of 20 μm, deionized water and anhydrous ethanol in a ratio of 50 g:100 mL:405 mL was uniformly performed to obtain a mixed solution A, and the pH value of the mixed solution A was adjusted to 5 using a 1 mol / L hydrochloric acid solution at a temperature of 55° C. to obtain a mixed solution B, and γ-aminopropyltriethoxysilane was added to the mixed solution B, and the mixture was stirred at a temperature of 60° C. for 5 h, and filtered, and the residue was washed with deionized water and anhydrous ethanol until the pH value was neutral, and the residue was dried at a temperature of 78° C., ground, and passed through a 270-mesh sieve to obtain modified sepiolite for later use; PC, TPU, SBS, PETG and potassium diphenyl sulfone-3 sulfonate were dried at a temperature of 2 h, respectively, and used for later use;

[0028] The mass ratio of the mixed solution B to γ-aminopropyltriethoxysilane is 1:0.12;

[0029] The temperature of the PC temperature-controlled drying is 115°C, the temperature of the TPU temperature-controlled drying is 75°C, the temperature of the SBS temperature-controlled drying is 80°C, the temperature of the PETG temperature-controlled drying is 100°C, and the temperature of the potassium diphenyl sulfone-3 sulfonate temperature-controlled drying is 110°C;

[0030] S2, HS i 6441P, RDP and sepiolite pretreated by S1, pretreated PC, pretreated TPU, pretreated SBS, pretreated PETG, and pretreated potassium diphenyl sulfone-3 sulfonate are uniformly mixed in a mass ratio of 1.8:5:12:75:12:3.8:25:0.002, placed in a twin-screw extruder for melt extrusion granulation, the particles obtained by extrusion granulation are dried at 80° C. for 4 h, and injection molded into strips by an injection molding machine at 230° C., which is a finished alloy material;

[0031] The extrusion temperature of each stage of the extrusion granulation is 210° C., and the screw speed is 200 r / min.

[0032] Example 2

[0033] A method for preparing a polycarbonate alloy, the preparation method specifically comprising the following steps:

[0034] S1, pre-treating sepiolite, PC, TPU, SBS, PETG and potassium diphenyl sulfone-3 sulfonate respectively, specifically:

[0035] Ultrasonic dispersion of sepiolite with a particle size of 10 μm, deionized water and anhydrous ethanol in a ratio of 52 g:105 mL:400 mL was uniformly performed to obtain a mixed solution A, and the pH value of the mixed solution A was adjusted to 5 using a 1 mol / L hydrochloric acid solution at a temperature of 60°C to obtain a mixed solution B, and γ-aminopropyltriethoxysilane was added to the mixed solution B, and the mixture was stirred at a temperature of 65°C for 6 hours, and filtered, and the filter residue was washed with deionized water and anhydrous ethanol until the pH value was neutral, and the mixture was dried at a temperature of 80°C, ground, and passed through a 250-mesh sieve to obtain modified sepiolite for later use; PC, TPU, SBS, PETG and potassium diphenyl sulfone-3 sulfonate were dried at a temperature of 2 hours respectively for later use;

[0036] The mass ratio of the mixed solution B to γ-aminopropyltriethoxysilane is 1:0.1;

[0037] The temperature of the PC temperature-controlled drying is 120°C, the temperature of the TPU temperature-controlled drying is 78°C, the temperature of the SBS temperature-controlled drying is 75°C, the temperature of the PETG temperature-controlled drying is 103°C, and the temperature of the potassium diphenyl sulfone-3 sulfonate temperature-controlled drying is 120°C;

[0038] S2, HS i 6441P, RDP and sepiolite pretreated by S1, pretreated PC, pretreated TPU, pretreated SBS, pretreated PETG, and pretreated potassium diphenyl sulfone-3 sulfonate are uniformly mixed in a mass ratio of 1:5.5:10:80:15:4:22.5:0.003, placed in a twin-screw extruder for melt extrusion granulation, the particles obtained by extrusion granulation are dried at 100° C. for 4 h, and injection molded into strips by an injection molding machine at 270° C., which is a finished alloy material;

[0039] The extrusion temperature of each stage of the extrusion granulation is 200° C., and the screw speed is 220 r / min.

[0040] Example 3

[0041] A method for preparing a polycarbonate alloy, the preparation method specifically comprising the following steps:

[0042] S1, pre-treating sepiolite, PC, TPU, SBS, PETG and potassium diphenyl sulfone-3 sulfonate respectively, specifically:

[0043] Ultrasonic dispersion of sepiolite with a particle size of 30 μm, deionized water and anhydrous ethanol in a ratio of 51 g:103 mL:410 mL was uniformly performed to obtain a mixed solution A, and the pH value of the mixed solution A was adjusted to 5 using a 1 mol / L hydrochloric acid solution at a temperature of 58°C to obtain a mixed solution B, and γ-aminopropyltriethoxysilane was added to the mixed solution B, and the mixture was stirred at a temperature of 63°C for 5 hours, and filtered, and the filter residue was washed with deionized water and anhydrous ethanol until the pH value was neutral, and the mixture was dried at a temperature of 75°C, ground, and passed through a 250-mesh sieve to obtain modified sepiolite for later use; PC, TPU, SBS, PETG and potassium diphenyl sulfone-3 sulfonate were dried at a temperature of 3 hours respectively for later use;

[0044] The mass ratio of the mixed solution B to γ-aminopropyltriethoxysilane is 1:0.11;

[0045] The temperature of the PC temperature-controlled drying is 118°C, the temperature of the TPU temperature-controlled drying is 80°C, the temperature of the SBS temperature-controlled drying is 70°C, the temperature of the PETG temperature-controlled drying is 105°C, and the temperature of the potassium diphenyl sulfone-3 sulfonate temperature-controlled drying is 115°C;

[0046] S2, HS i 6441P, RDP and sepiolite pretreated by S1, pretreated PC, pretreated TPU, pretreated SBS, pretreated PETG, and pretreated potassium diphenyl sulfone-3 sulfonate are uniformly mixed in a mass ratio of 2.5:6:11:85:13.5:4.2:20:0.004, placed in a twin-screw extruder for melt extrusion granulation, the particles obtained by extrusion granulation are dried at 90° C. for 5 h, and injection molded into strips by an injection molding machine at 250° C., which is a finished alloy material;

[0047] The extrusion temperature of each stage of the extrusion granulation is 220° C., and the screw speed is 210 r / min.

[0048] Comparative Example 1

[0049] Compared with Example 3, the difference is that in step S2 of comparative example 1, HS i 6441P is not added, that is, the mass ratio of RDP, sepiolite pretreated by S1, pretreated PC, pretreated TPU, pretreated SBS, pretreated PETG, and pretreated potassium diphenyl sulfone-3 sulfonate is 6:11:85:14.3:5.1:20.8:0.004, and the other operating steps and parameters remain unchanged.

[0050] Comparative Example 2

[0051] Compared with Example 3, the difference is that in step S2 of Comparative Example 2, the pretreated TPU is not added, that is, the mass ratio of HS i6441P, RDP and sepiolite pretreated by S1, pretreated PC, pretreated SBS, pretreated PETG, and pretreated potassium diphenyl sulfone-3 sulfonate is 7:6:11:85:8.7:24.5:0.004, and the other operating steps and parameters remain unchanged.

[0052] Comparative Example 3

[0053] Compared with Example 3, the difference is that in step S2 of comparative example 3, no pretreated SBS is added, that is, the mass ratio of HS i6441P, RDP and sepiolite pretreated by S1, pretreated PC, pretreated TPU, pretreated PETG, and pretreated potassium diphenyl sulfone-3 sulfonate is 3.9:6:11:85:14.9:21.4:0.004, and the other operating steps and parameters remain unchanged.

[0054] Comparative Example 4

[0055] Compared with Example 3, the difference is that in step S2 of Comparative Example 4, the pretreated PETG is not added, that is, the mass ratio of HS i6441P, RDP and sepiolite pretreated by S1, pretreated PC, pretreated TPU, pretreated SBS, and pretreated potassium diphenyl sulfone-3 sulfonate is 9.3:6:11:85:20.1:10.8:0.004, and the other operating steps and parameters remain unchanged.

[0056] Comparative Example 5

[0057] Compared with Example 3, the difference is that in step S2 of Comparative Example 5, pretreated potassium diphenyl sulfone-3-sulfonate is not added, and the other operating steps and parameters remain unchanged.

[0058] Comparative Example 6

[0059] Compared with Example 3, the difference is that RDP is not added in step S2 of Comparative Example 6, and the other operation steps and parameters remain unchanged.

[0060] Comparative Example 7

[0061] Compared with Example 3, the difference is that in step S2 of Comparative Example 7, no pretreated sepiolite is added, and the other operating steps and parameters remain unchanged.

[0062] Test Case

[0063] (1) Solvent resistance test: According to standard ASTM D543, peanut oil (brand: Orchid) was applied to a tensile strength test specimen (test specimen thickness 3.2 mm) in a 1.0% strain fixture and the appearance change was observed. The test specimen was divided into four grades according to the severity of the cracks: A (no cracks), B (cracks, cracks that do not penetrate the specimen and are discontinuous when observed by the naked eye, and the crack length is less than or equal to 3 mm), C (severe cracks, through- or continuous cracks observed by the naked eye, and the length is greater than 3 mm) and D (fracture); the solvent resistance of the finished alloy materials obtained in Examples 1-3 and Comparative Examples 1-4 was judged in this way, and the results are shown in Table 1.

[0064] (2) Wear resistance test: According to standard GB / T 3960-83, the finished alloy materials obtained in Examples 1-3 and Comparative Examples 1-4 were tested for wear coefficient. The larger the wear coefficient, the faster the wear rate. The results are shown in Table 1.

[0065] (3) Flame retardant performance test: According to standard UL94-2021, the finished alloy materials obtained in Examples 1-3 and Comparative Examples 5-7 were injection molded into 0.8 mm combustion specimens, and the combustion performance was tested using a combustion box. The results are shown in Table 1.

[0066] Table 1

[0067] Solvent resistance (grade) <![CDATA[Wear coefficient (mm 3 / kg / km)]]> Flame retardant grade Example 1 A 6.5 V-0 Example 2 A 6.2 V-0 Example 3 A 5.8 V-0 Comparative Example 1 B 9.9 —— Comparative Example 2 C 8.0 —— Comparative Example 3 B 8.9 —— Comparative Example 4 C 9.3 —— Comparative Example 5 —— —— V-2 Comparative Example 6 —— —— V-2 Comparative Example 7 —— —— V-1

[0068] It can be seen from the data of Examples 1-3 and Comparative Examples 1-4 in Table 1 that the finished alloy material prepared by the present invention has outstanding chemical solvent resistance and wear resistance. This is because the present invention selects PC as the main base material to provide better toughness, and breaks through the use of TPU, SBS, H-SI6441P and PETG as the base material of the blended alloy material, making full use of the advantages of the performance of the four different raw materials, complementing each other's strengths, and synergistically making the finished alloy material have excellent solvent resistance and wear resistance.

[0069] It can be seen from the data of Examples 1-3 and Comparative Examples 5-7 in Table 1 that the finished alloy material prepared by the present invention has excellent flame retardant properties. Specifically, because the potassium diphenyl sulfone-3 sulfonate added in the present invention can effectively form a carbon layer, the added RDP can effectively prevent the combustion chain reaction from proceeding, and the added sepiolite can further increase the density of the system to form a carbon layer, therefore, the finished alloy material prepared thereby has excellent flame retardant properties.

[0070] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0071] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a polycarbonate alloy, characterized in that: The preparation method specifically comprises the following steps: S1, pre-treating sepiolite, PC, TPU, SBS, PETG and potassium diphenyl sulfone-3 sulfonate respectively; S2, the functional additives, RDP and pretreated sepiolite, PC, TPU, SBS, PETG, potassium biphenyl sulfone-3 sulfonate are uniformly mixed, placed in a twin-screw extruder for melt extrusion granulation, the particles obtained by extrusion granulation are temperature-controlled dried and injection-molded into strips by an injection molding machine under temperature control, i.e., a finished alloy material; The mass ratio of the functional additive, RDP, pretreated sepiolite, pretreated PC, pretreated TPU, pretreated SBS, pretreated PETG, and pretreated potassium diphenyl sulfone-3 sulfonate is 1-2.5:5-6:10-12:75-85:12-15:3.8-4.2:20-25:0.002-0.004; The functional additive is a functional additive of EVONIK brand H-Si 6441P; The step S1 specifically comprises: uniformly dispersing sepiolite, deionized water and anhydrous ethanol by ultrasonication to obtain a mixed solution A, adjusting the pH of the mixed solution A by temperature control to obtain a mixed solution B, adding γ-aminopropyltriethoxysilane to the mixed solution B by temperature control and stirring, filtering by suction, washing the filter residue, drying by temperature control, grinding and sieving to obtain the modified sepiolite for later use; and drying PC, TPU, SBS, PETG and potassium diphenyl sulfone-3 sulfonate by temperature control and for later use.

2. The method for preparing a polycarbonate alloy according to claim 1, characterized in that: The usage ratio of the sepiolite, deionized water and anhydrous ethanol is 50-52 g:100-105 mL:400-410 mL; the mass ratio of the mixed solution B and γ-aminopropyltriethoxysilane is 1:0.1-0.

12.

3. The method for preparing a polycarbonate alloy according to claim 1, characterized in that: The particle size of the sepiolite is 10-30 μm.

4. The method for preparing a polycarbonate alloy according to claim 1, characterized in that: The temperature-controlled adjustment of the pH of the mixed solution A is to control the temperature at 55-60°C and use 1 mol / L hydrochloric acid solution to adjust the pH of the mixed solution A to 5; the temperature of the temperature-controlled stirring is 60-65°C, and the time is 5-6h; the filter residue washing is to wash the filter residue with deionized water and anhydrous ethanol until the pH is neutral; the temperature of the modified sepiolite temperature-controlled drying is 75-80°C; and the screening is to pass through a 250-270 mesh sieve.

5. The method for preparing a polycarbonate alloy according to claim 1, characterized in that: In step S1, the temperature of PC temperature-controlled drying is 115-120°C, the temperature of TPU temperature-controlled drying is 75-80°C, the temperature of SBS temperature-controlled drying is 70-80°C, the temperature of PETG temperature-controlled drying is 100-105°C, and the temperature of potassium diphenyl sulfone-3 sulfonate temperature-controlled drying is 110-120°C; the drying time of PC, TPU, SBS, PETG and potassium diphenyl sulfone-3 sulfonate is 2-3h.

6. The method for preparing a polycarbonate alloy according to claim 1, characterized in that: In step S2, the extrusion temperature of each section of the extrusion granulation is 200-220°C, and the screw speed is 200-220r / min; the temperature of the temperature-controlled drying is 80-100°C, and the time is 4-5h; the temperature of the temperature-controlled injection molding into the spline is 230-270°C.

7. A polycarbonate alloy prepared by the method for preparing a polycarbonate alloy according to any one of claims 1 to 6.

8. Use of the polycarbonate alloy as claimed in claim 7 in the manufacture of automobile parts, electronic and electrical products, office equipment products, packaging materials, and building materials.