A preparation method of epoxy potting glue for chip packaging

By modifying hexagonal boron nitride and phosphorus-based flame retardant, activated thermal fillers and reactive flame retardants are formed, which solves the problem of insufficient thermal conductivity and flame retardant performance of existing epoxy potting glues, and achieves efficient thermal conductivity and flame retardant performance improves.

CN118496789BActive Publication Date: 2024-11-19YAHAI NEW MATERIAL TECH (SHANDONG) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410755289.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-11-19
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

When existing epoxy potting adhesives improve thermal conductivity and flame retardant properties, the modification process of hexagonal boron nitride is likely to cause B-N bonds to break, affecting thermal conductivity, and the cross-linking density of phosphorus-based flame retardants and epoxy resins is reduced, which affects the Mechanics and heat resistance.

Method used

Thermal filler is prepared by introducing hydroxyl and amino groups into hexagonal boron nitride to form activated hexagonal boron nitride and hydrolyzed with γ-aminopropyltriethoxysilane; the reactive flame retardant is prepared by using DOPO and Schiff-containing alkali structures to prepare a Reduce the capping effect and enhance the crosslinking structure.

Benefits of technology

The thermal conductivity and flame retardant properties of epoxy potting adhesive are improved, the thermal conductivity coefficient is ≥1.4, the limit oxygen index is ≥37%, and the flame retardant level reaches V-0, enhancing mechanical and high temperature resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention discloses a method for preparing epoxy potting glue for chip encapsulation, which belongs to the technical field of epoxy glue, and comprises the following steps: adding a flame retardant to an epoxy resin, stirring and mixing, then adding a thermally conductive filler, a diluent and a toughening agent thereto, stirring and mixing, then adding a dispersant, a defoamer and a coupling agent thereto, stirring and mixing, vacuumizing after the stirring is completed, and continuing to stir and mix to obtain component A; stirring and mixing an epoxy curing agent and an accelerator, vacuumizing after the stirring is completed, and continuing to stir and mix to obtain component B; stirring and mixing component A and component B, and after stirring and mixing, obtaining epoxy potting glue for chip encapsulation. The present invention improves the thermal conductivity and flame retardancy of the epoxy potting glue by improving the thermally conductive filler and the flame retardant. The thermal conductivity coefficient of the epoxy potting glue prepared by the present invention is ≥1.4 (w / (m·k); 25°C), the limiting oxygen index is ≥37%, and the flame retardancy level reaches V‑0.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of epoxy adhesives, and in particular relates to a method for preparing epoxy potting adhesive for chip packaging. Background Art

[0002] Chips are core components of electronic products, so the selection of packaging materials is particularly critical. Epoxy potting adhesives are widely used in the field of chip packaging due to their excellent moisture-proof, shock-proof, heat-insulating, anti-friction and insulation properties. With the continuous improvement of chip integration, the demand for thermal conductivity and flame retardancy of epoxy potting adhesives continues to increase. In the existing technology, thermal conductivity and flame retardancy are improved by adding thermal conductive fillers and flame retardants to epoxy resins. Among them, hexagonal boron nitride is a commonly used thermal conductive filler, and phosphorus-based flame retardants are the flame retardant systems that are currently being studied more deeply.

[0003] Hexagonal boron nitride has high thermal conductivity, low dielectric constant, excellent thermal stability and electrical insulation, but its surface lacks sufficient active functional groups, which limits its wide application. In the prior art, hexagonal boron nitride is often modified by mechanochemical methods such as ball milling, mainly to form hydroxyl groups on the B atom. However, the ball milling process will cause the BN bonds in the hexagonal boron nitride to break. If other active functional groups exist during the ball milling process, they will directly react with the sites on B and N, causing the hexagonal boron nitride structure to be destroyed and the thermal conductivity to be significantly reduced.

[0004] Phosphorus-based flame retardants have excellent flame retardancy and stability. Among them, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is widely used in epoxy resin systems as a high-efficiency phosphorus-containing flame retardant. However, the introduction of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide will have a capping effect with the epoxy groups in the epoxy resin, thereby reducing the cross-linking density of the epoxy resin and causing a significant decrease in the glass transition temperature of the epoxy resin, thereby affecting the mechanical properties and heat resistance of the finally prepared epoxy resin potting compound. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing epoxy potting glue for chip packaging, and to improve the thermal conductivity and flame retardancy of the epoxy potting glue by improving the thermal conductive filler and the flame retardant.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing epoxy potting glue for chip packaging comprises the following steps:

[0008] S1, adding a flame retardant to the epoxy resin, stirring and mixing, then adding a thermal conductive filler, a diluent and a toughening agent thereto, stirring and mixing, then adding a dispersant, a defoaming agent and a coupling agent thereto, stirring and mixing, after stirring is completed, evacuating, and continuing to stir and mix to obtain component A;

[0009] S2, stirring and mixing the epoxy curing agent and the accelerator, after stirring, evacuating, and continuing to stir and mix to obtain component B;

[0010] S3, stirring and mixing component A and component B, and after stirring and mixing, obtaining epoxy potting adhesive for chip packaging.

[0011] Furthermore, the mass ratio of the epoxy resin, thermal conductive filler, flame retardant, diluent, toughening agent, dispersant, defoaming agent and coupling agent in S1 is 37-40:15-20:4-7:3-4:12-15:1-2:1-2:1-2.

[0012] Furthermore, the brand of the epoxy resin is DER-331; the diluent is polyethylene glycol glycidyl dodecyl ether; the toughening agent is WD-401 toughening agent; the dispersant is dispersant BYK-W980; the defoaming agent is one of defoaming agent BYK-054 and defoaming agent BYK-057; and the coupling agent is a mixture of silane coupling agent KH-560 and titanate coupling agent JTW-201 in a mass ratio of 3 to 4:1 to 2.

[0013] Furthermore, the mass ratio of the epoxy curing agent to the accelerator in S2 is 10:0.5-1.0.

[0014] Furthermore, the epoxy curing agent is prepared by mixing methyltetrahydrophthalic anhydride and methylnadic anhydride in a mass ratio of 9.0 to 9.5:1; and the accelerator is one of 2-ethylimidazole and 2-ethyl-4-methylimidazole.

[0015] Furthermore, the mass ratio of component A to component B in S3 is 5 to 6:1.

[0016] Furthermore, the thermally conductive filler is prepared by the following steps:

[0017] A1: Chloroform and sulfonyl chloride are mixed to obtain an activation solution, hexagonal boron nitride is added to the activation solution with stirring, and then ultrasonic stirring is performed for 48 hours at room temperature. After the ultrasonic stirring is completed, vacuum filtration is performed, and the solid component is washed three times with dichloromethane, and then dried at 80-100°C for 12 hours to obtain activated hexagonal boron nitride;

[0018] A2: Add γ-aminopropyltriethoxysilane to toluene with stirring, heat to 80-100°C, stir at constant temperature for 30 min, then drop deionized water into the mixture, reflux and hydrolyze for 2-4 h, and after the reflux and hydrolysis is completed, purify and remove the generated ethanol and unreacted deionized water to obtain a silanol mixed solvent;

[0019] A3: Add activated hexagonal boron nitride to toluene with stirring, ultrasonically disperse for 1 to 2 hours, then add silanol mixed solvent with stirring, stir and mix for 10 to 20 minutes, then add 18% by mass dilute hydrochloric acid to adjust the pH of the system to 6.0 to 6.5, heat the system to 112 to 115°C, reflux for 4 to 5 hours, cool to room temperature after the reflux reaction, filter, take the solid component, wash it with anhydrous ethanol and deionized water, and then dry it under vacuum conditions at 80 to 100°C for 2 to 4 hours to obtain a thermal conductive filler.

[0020] Furthermore, the volume ratio of chloroform and sulfuryl chloride in A1 is 1:1.

[0021] Furthermore, the usage ratio of the activation solution and hexagonal boron nitride in A1 is 200 mL:50.0 g; the usage ratio of toluene, γ-aminopropyltriethoxysilane and deionized water in A2 is 100 mL:20 mL:8-10 mL; the usage ratio of toluene, activated hexagonal boron nitride and silanol mixed solvent in A3 is 100 mL:20 g:80-100 mL.

[0022] Furthermore, the flame retardant is prepared by the following steps:

[0023] B1: Take chloroform, add vanillin, triethylamine and phosphorus oxychloride to it under nitrogen protection, stir until the solid is completely dissolved, then heat to 40-50°C, stir and react for 24 hours. After the reaction is completed, cool to room temperature, filter, wash the filtrate three times with saturated brine, and then concentrate and crystallize to obtain intermediate 1. The preparation process of intermediate 1 is as follows: .

[0024] B2: Take anhydrous ethanol, add intermediate 1 and ethanolamine to it under nitrogen protection, stir until the solid is completely dissolved, then heat to 50-55°C, stir and react for 4-5 hours. After the reaction is completed, cool to room temperature, and remove anhydrous ethanol by rotary evaporation to obtain intermediate 2. The preparation process of intermediate 2 is as follows: .

[0025] B3: Take 1,4-dioxane, add intermediate II and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide under nitrogen protection, and heat to 70-75°C, stir and react for 4-5 hours. After the reaction is completed, cool to room temperature, filter, take the solid component and wash it three times with 1,4-dioxane to obtain a flame retardant. The preparation process of the flame retardant is as follows: .

[0026] Furthermore, the dosage ratio of chloroform, vanillin, triethylamine and phosphorus oxychloride described in B1 is 200 mL: 0.2 mol: 0.2 mol: 0.1 mol; the dosage ratio of anhydrous ethanol, intermediate 1 and ethanolamine described in B2 is 100 mL: 0.1 mol: 0.1 mol; the dosage ratio of 1,4-dioxane, intermediate 2 and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide described in B3 is 100 mL: 0.1 mol: 0.2 mol.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The present invention provides a method for preparing an epoxy potting adhesive for chip packaging. The epoxy potting adhesive prepared by the present invention has excellent thermal conductivity and flame retardancy. After testing, the thermal conductivity of the epoxy potting adhesive prepared by the present invention is ≥1.4 (w / (m•k); 25°C), the limiting oxygen index is ≥37%, and the flame retardancy level reaches V-0. Specifically, the present invention improves the thermal conductive filler and the flame retardant, and the specific advantages are as follows:

[0029] 1. The thermal conductive filler prepared by the present invention has the following advantages:

[0030] First, the present invention utilizes acyl chloride to corrode hexagonal boron nitride and introduces a large number of hydroxyl groups and amino groups on its surface to obtain activated hexagonal boron nitride. The above activation process helps to improve the compatibility between hexagonal boron nitride and epoxy resin and other substrates, thereby helping to form dense and uniform heat conduction paths in the epoxy potting compound, thereby helping to improve the thermal conductivity of the epoxy potting compound.

[0031] At the same time, the present invention further utilizes the hydroxyl groups on the activated hexagonal boron nitride and the hydroxyl groups of the silanol after the hydrolysis of γ-aminopropyltriethoxysilane to carry out dehydration condensation, and introduces a silicon-philic aminosilanol structure into the activated hexagonal boron nitride to obtain a thermally conductive filler. The aminosilanol structure of the thermally conductive filler can form a silicon-oxygen-silicon bond with the surface of the semiconductor silicon wafer in the chip during packaging, which helps to improve the adhesion between the finally prepared epoxy potting adhesive and the chip during the chip potting process.

[0032] Then, the amino groups on the hexagonal boron nitride in the thermal conductive filler and the amino groups in the aminosilanol structure can form amino-silicon bonds with the surface of the semiconductor silicon wafer. At the same time, they can form coordination bonds with metal materials such as the pins on the chip, further improving the adhesion of the epoxy potting adhesive to the chip during the chip potting process.

[0033] Finally, the amino group in the thermally conductive filler can undergo an epoxy-amino ring-opening reaction with the base epoxy resin under high temperature conditions, which can improve the bonding performance between the thermally conductive filler and the epoxy resin base under high temperature conditions, thereby helping to ensure the stability of the thermal conductivity of the epoxy potting compound under high temperature conditions.

[0034] Second, the flame retardant prepared by the present invention has the following advantages:

[0035] Firstly, the flame retardant prepared by the present invention is prepared from DOPO and an intermediate II containing a Schiff base structure, and the PH bond of DOPO is reacted with the C=N of the Schiff base intermediate II. The flame retardant finally prepared belongs to a reactive flame retardant, which realizes high-efficiency flame retardancy through gas phase flame retardancy (nitrogen elements form inert gases to inhibit combustion), heat absorption, chemical extinguishing (phosphorus and nitrogen elements react with free radicals to prevent the propagation of the combustion chain) and the formation of a dense carbon layer residue. The flame retardant prepared by the present invention has the flame retardant properties of both phosphorus-based flame retardants and nitrogen-based flame retardants, gives full play to the flame retardancy of the gas phase and the condensed phase, and comprehensively realizes the improvement of flame retardant performance.

[0036] Then, the present invention utilizes the C=N containing Schiff base intermediate II to react with the PH bond of DOPO, thereby reducing the end-capping effect of the subsequent epoxy resin. At the same time, the flame retardant prepared by the present invention has multiple rigid benzene ring structures, which can comprehensively improve the mechanical properties and high temperature resistance of the epoxy potting glue.

[0037] Finally, the flame retardant prepared by the present invention contains secondary amine groups, which react with the epoxy groups of the epoxy resin to generate oxyamino intermediates, and the oxyamino groups react with the epoxy groups of other epoxy resin molecules to form a cross-linked structure between the epoxy resin molecules. This cross-linked structure can increase the mechanical properties, heat resistance and chemical stability of the epoxy resin, and at the same time can "anchor" the flame retardant in the epoxy resin matrix, thereby improving the compatibility of the flame retardant with the epoxy resin, thereby improving the high temperature resistance of the finally prepared epoxy potting glue. DETAILED DESCRIPTION

[0038] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Example 1

[0040] Preparation of thermally conductive fillers:

[0041] Activation of hexagonal boron nitride: Chloroform and sulfuryl chloride were mixed in a volume ratio of 1:1 to obtain an activation solution. 50.0 g of hexagonal boron nitride was added to 200 mL of the activation solution with stirring, and then ultrasonic stirring was carried out for 48 h at room temperature. After the ultrasonic stirring and mixing were completed, vacuum filtration was performed, and the solid component was washed three times with dichloromethane, and then dried at 80°C for 12 h to obtain activated hexagonal boron nitride.

[0042] Silane hydrolysis: add 20 mL of γ-aminopropyltriethoxysilane to 100 mL of toluene with stirring, heat to 80°C, stir at constant temperature for 30 min, then add 8 mL of deionized water dropwise, reflux hydrolyze for 2 h. After the reflux hydrolysis is completed, purify and remove the generated ethanol and unreacted deionized water to obtain a silanol mixed solvent.

[0043] Preparation of thermal conductive filler: Add 20 g of activated hexagonal boron nitride to 100 mL of toluene with stirring, ultrasonically disperse for 1 hour, then add 80 mL of silanol mixed solvent with stirring, stir and mix for 10 minutes, then add 18% by mass dilute hydrochloric acid to adjust the pH of the system to 6.0, heat the system to 112°C, reflux for 4 hours, cool to room temperature after the reflux reaction, filter, take the solid component, wash it with anhydrous ethanol and deionized water, and then dry it under vacuum at 80°C for 2 hours to obtain a thermal conductive filler.

[0044] Example 2

[0045] Preparation of thermally conductive fillers:

[0046] Activation of hexagonal boron nitride: Chloroform and sulfuryl chloride were mixed in a volume ratio of 1:1 to obtain an activation solution. 50.0 g of hexagonal boron nitride was added to 200 mL of the activation solution with stirring, and then ultrasonic stirring was carried out for 48 h at room temperature. After the ultrasonic stirring was completed, vacuum filtration was performed, and the solid component was washed three times with dichloromethane, and then dried at 90°C for 12 h to obtain activated hexagonal boron nitride.

[0047] Silane hydrolysis: add 20 mL of γ-aminopropyltriethoxysilane to 100 mL of toluene with stirring, heat to 90°C, stir at constant temperature for 30 min, then add 9 mL of deionized water dropwise, reflux hydrolysis for 4 h. After the reflux hydrolysis is completed, purify and remove the generated ethanol and unreacted deionized water to obtain a silanol mixed solvent.

[0048] Preparation of thermal conductive filler: Add 20 g of activated hexagonal boron nitride to 100 mL of toluene with stirring, ultrasonically disperse for 2 hours, then add 90 mL of silanol mixed solvent with stirring, stir and mix for 20 minutes, then add 18% by mass dilute hydrochloric acid to adjust the pH of the system to 6.4, heat the system to 114°C, reflux for 5 hours, cool to room temperature after the reflux reaction, filter, take the solid component, wash it with anhydrous ethanol and deionized water, and then dry it at 900°C under vacuum conditions for 4 hours to obtain a thermal conductive filler.

[0049] Example 3

[0050] Preparation of thermally conductive fillers:

[0051] Activation of hexagonal boron nitride: Chloroform and sulfuryl chloride were mixed in a volume ratio of 1:1 to obtain an activation solution. 50.0 g of hexagonal boron nitride was added to 200 mL of the activation solution with stirring, and then ultrasonic stirring was carried out for 48 h at room temperature. After the ultrasonic stirring and mixing were completed, vacuum filtration was performed, and the solid component was washed three times with dichloromethane, and then dried at 100°C for 12 h to obtain activated hexagonal boron nitride.

[0052] Silane hydrolysis: add 20 mL of γ-aminopropyltriethoxysilane to 100 mL of toluene with stirring, heat to 100°C, stir at constant temperature for 30 min, then add 10 mL of deionized water dropwise, reflux hydrolysis for 4 h. After the reflux hydrolysis is completed, purify and remove the generated ethanol and unreacted deionized water to obtain a silanol mixed solvent.

[0053] Preparation of thermal conductive filler: Add 20 g of activated hexagonal boron nitride to 100 mL of toluene with stirring, ultrasonically disperse for 2 hours, then add 100 mL of silanol mixed solvent with stirring, stir and mix for 20 minutes, then add 18% by mass dilute hydrochloric acid to adjust the pH of the system to 6.5, heat the system to 115°C, reflux for 5 hours, cool to room temperature after the reflux reaction, filter, take the solid component, wash it with anhydrous ethanol and deionized water, and then dry it under vacuum conditions at 100°C for 4 hours to obtain a thermal conductive filler.

[0054] Example 4

[0055] Preparation of flame retardant:

[0056] Preparation of intermediate 1: Take 200 mL of chloroform, add 0.2 mol of vanillin, 0.2 mol of triethylamine and 0.1 mol of phosphorus oxychloride thereto with stirring under nitrogen protection, stir until the solid is completely dissolved, then heat to 40°C, stir and react for 24 h. After the reaction is completed, cool to room temperature, filter, wash the filtrate three times with saturated brine, and then concentrate and crystallize to obtain intermediate 1.

[0057] Preparation of intermediate 2: Take 100 mL of anhydrous ethanol, under nitrogen protection, add 0.1 mol of intermediate 1 and 0.1 mol of ethanolamine, stir until the solid is completely dissolved, then heat to 50°C, stir and react for 4 h. After the reaction is completed, cool to room temperature, and remove anhydrous ethanol by rotary evaporation to obtain intermediate 2.

[0058] Preparation of flame retardant: Take 100 mL of 1,4-dioxane, under nitrogen protection, add 0.1 mol of intermediate II and 0.2 mol of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and then heat to 70°C and stir to react for 4 hours. After the reaction is completed, cool to room temperature, filter, and wash the solid component three times with 1,4-dioxane to obtain a flame retardant.

[0059] Example 5

[0060] Preparation of flame retardant:

[0061] Preparation of intermediate 1: Take 200 mL of chloroform, add 0.2 mol of vanillin, 0.2 mol of triethylamine and 0.1 mol of phosphorus oxychloride thereto with stirring under nitrogen protection, stir until the solid is completely dissolved, then heat to 45°C, stir and react for 24 h. After the reaction is completed, cool to room temperature, filter, wash the filtrate three times with saturated brine, and then concentrate and crystallize to obtain intermediate 1.

[0062] Preparation of intermediate 2: Take 100 mL of anhydrous ethanol, add 0.1 mol of intermediate 1 and 0.1 mol of ethanolamine under nitrogen protection, stir until the solid is completely dissolved, then heat to 54°C, stir and react for 5 h. After the reaction is completed, cool to room temperature, and remove anhydrous ethanol by rotary evaporation to obtain intermediate 2.

[0063] Preparation of flame retardant: Take 100 mL of 1,4-dioxane, under nitrogen protection, add 0.1 mol of intermediate II and 0.2 mol of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and then heat to 74 ° C, stir and react for 5 hours. After the reaction is completed, cool to room temperature, filter, take the solid component and wash it three times with 1,4-dioxane to obtain a flame retardant.

[0064] Example 6

[0065] Preparation of flame retardant:

[0066] Preparation of intermediate 1: Take 200 mL of chloroform, add 0.2 mol of vanillin, 0.2 mol of triethylamine and 0.1 mol of phosphorus oxychloride under nitrogen protection, stir until the solid is completely dissolved, then heat to 50°C, stir and react for 24 h. After the reaction is completed, cool to room temperature, filter, wash the filtrate three times with saturated brine, and then concentrate and crystallize to obtain intermediate 1.

[0067] Preparation of intermediate 2: Take 100 mL of anhydrous ethanol, under nitrogen protection, add 0.1 mol of intermediate 1 and 0.1 mol of ethanolamine, stir until the solid is completely dissolved, then heat to 55°C, stir and react for 5 h. After the reaction is completed, cool to room temperature, and remove anhydrous ethanol by rotary evaporation to obtain intermediate 2.

[0068] Preparation of flame retardant: Take 100 mL of 1,4-dioxane, under nitrogen protection, add 0.1 mol of intermediate II and 0.2 mol of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and then heat to 75°C and stir to react for 5 hours. After the reaction is completed, cool to room temperature, filter, take the solid component and wash it three times with 1,4-dioxane to obtain a flame retardant.

[0069] Example 7

[0070] Preparation of epoxy potting compound for chip packaging:

[0071] Raw material components: Epoxy potting glue for chip encapsulation is made by mixing component A and component B;

[0072] Component A includes the following components by mass: 37 parts of epoxy resin, 15 parts of thermal conductive filler prepared in Example 1, 4 parts of flame retardant prepared in Example 4, 3 parts of diluent, 12 parts of toughening agent, 1 part of dispersant, 1 part of defoaming agent, and 1 part of coupling agent; wherein the brand of epoxy resin is DER-331, which is purchased from Dow Chemical Company; wherein the diluent is polyethylene glycol glycidyl dodecyl ether, which is purchased from Sinopharm Chemical Reagent Co., Ltd.; wherein the toughening agent is WD-401 toughening agent, which is purchased from Guangzhou Good New Material Technology Co., Ltd.; wherein the dispersant is dispersant BYK-W980, and the defoaming agent is defoaming agent BYK-054, which are purchased from BYK Additives (Shanghai) Co., Ltd.; wherein the coupling agent is a mixture of silane coupling agent KH-560 and titanate coupling agent JTW-201 in a mass ratio of 3:1, and both are purchased from Nanjing Jingtianwei Chemical Co., Ltd.

[0073] In parts by mass, component B includes the following components: 10 parts of epoxy curing agent and 0.5 parts of accelerator; wherein, the epoxy curing agent is a mixture of methyltetrahydrophthalic anhydride and methylnadic anhydride in a mass ratio of 9.0:1, methyltetrahydrophthalic anhydride (purity 99%) is purchased from Sinopharm Chemical Reagent Co., Ltd., and methylnadic anhydride (purity 95%) is purchased from Sinopharm Chemical Reagent Co., Ltd.; wherein, the accelerator is 2-ethylimidazole, which is purchased from Sinopharm Chemical Reagent Co., Ltd.

[0074] Preparation of component A: Weigh the raw materials of component A by mass, add the flame retardant prepared in Example 4 to the epoxy resin, stir and mix for 20 min, then add the thermal conductive filler, diluent and toughening agent prepared in Example 1, stir and mix for 30 min, then add the dispersant, defoamer and coupling agent, stir and mix for 10 min, after stirring, evacuate to -0.09 MPa, continue to stir and mix for 40 min, and obtain component A.

[0075] Preparation of component B: Weigh the raw materials of component B according to mass parts, stir and mix the epoxy curing agent and the accelerator for 5 minutes, and after stirring, evacuate to -0.09 Mpa, continue to stir and mix for 20 minutes to obtain component B.

[0076] Preparation of epoxy potting glue for chip encapsulation: Component A and component B are stirred and mixed at a speed of 1000 r / min for 3 minutes, wherein the mass ratio of component A to component B is 5:1. After stirring and mixing, the epoxy potting glue for chip encapsulation is obtained.

[0077] Example 8

[0078] Preparation of epoxy potting compound for chip packaging:

[0079] Raw material components: Epoxy potting glue for chip encapsulation is made by mixing component A and component B;

[0080] Component A includes the following components by mass: 38 parts of epoxy resin, 18 parts of thermal conductive filler prepared in Example 2, 6 parts of flame retardant prepared in Example 5, 4 parts of diluent, 14 parts of toughening agent, 1 part of dispersant, 1 part of defoaming agent, and 1 part of coupling agent; wherein the brand of epoxy resin is DER-331, which is purchased from Dow Chemical Company; wherein the diluent is polyethylene glycol glycidyl dodecyl ether, which is purchased from Sinopharm Chemical Reagent Co., Ltd.; wherein the toughening agent is WD-401 toughening agent, which is purchased from Guangzhou Good New Material Technology Co., Ltd.; wherein the dispersant is dispersant BYK-W980, and the defoaming agent is defoaming agent BYK-057, which are purchased from BYK Additives (Shanghai) Co., Ltd.; wherein the coupling agent is a mixture of silane coupling agent KH-560 and titanate coupling agent JTW-201 in a mass ratio of 4:1, and both are purchased from Nanjing Jingtianwei Chemical Co., Ltd.

[0081] In parts by mass, component B includes the following components: 10 parts of epoxy curing agent and 0.8 parts of accelerator; wherein, the epoxy curing agent is a mixture of methyltetrahydrophthalic anhydride and methylnadic anhydride in a mass ratio of 9.2:1, methyltetrahydrophthalic anhydride (purity 99%) is purchased from Sinopharm Chemical Reagent Co., Ltd., and methylnadic anhydride (purity 95%) is purchased from Sinopharm Chemical Reagent Co., Ltd.; wherein, the accelerator is 2-ethyl-4-methylimidazole, both of which are purchased from Sinopharm Chemical Reagent Co., Ltd.

[0082] Preparation of component A: Weigh the raw materials of component A by mass, add the flame retardant prepared in Example 5 to the epoxy resin, stir and mix for 30 min, then add the thermal conductive filler, diluent and toughening agent prepared in Example 2, stir and mix for 40 min, then add the dispersant, defoamer and coupling agent, stir and mix for 20 min, after stirring, evacuate to -0.08 MPa, continue to stir and mix for 50 min, and obtain component A.

[0083] Preparation of component B: Weigh the raw materials of component B according to mass parts, stir and mix the epoxy curing agent and the accelerator for 6 minutes, and after stirring, evacuate to -0.08 Mpa, continue to stir and mix for 25 minutes to obtain component B.

[0084] Preparation of epoxy potting adhesive for chip encapsulation: Component A and component B are stirred and mixed at a rotation speed of 1200 r / min for 4 minutes, wherein the mass ratio of component A to component B is 6:1. After stirring and mixing, the epoxy potting adhesive for chip encapsulation is obtained.

[0085] Example 9

[0086] Preparation of epoxy potting compound for chip packaging:

[0087] Raw material components: Epoxy potting glue for chip encapsulation is made by mixing component A and component B;

[0088] Component A includes the following components by mass: 37 parts of epoxy resin, 20 parts of thermal conductive filler prepared in Example 3, 7 parts of flame retardant prepared in Example 7, 4 parts of diluent, 15 parts of toughening agent, 2 parts of dispersant, 2 parts of defoaming agent, and 2 parts of coupling agent; wherein the brand of epoxy resin is DER-331, which is purchased from Dow Chemical Company; wherein the diluent is polyethylene glycol glycidyl dodecyl ether, which is purchased from Sinopharm Chemical Reagent Co., Ltd.; wherein the toughening agent is WD-401 toughening agent, which is purchased from Guangzhou Good New Material Technology Co., Ltd.; wherein the dispersant is dispersant BYK-W980, and the defoaming agent is defoaming agent BYK-057, which are purchased from BYK Additives (Shanghai) Co., Ltd.; wherein the coupling agent is a mixture of silane coupling agent KH-560 and titanate coupling agent JTW-201 in a mass ratio of 2:1, and both are purchased from Nanjing Jingtianwei Chemical Co., Ltd.

[0089] In parts by mass, component B includes the following components: 10 parts of epoxy curing agent and 1.0 part of accelerator; wherein, the epoxy curing agent is a mixture of methyltetrahydrophthalic anhydride and methylnadic anhydride in a mass ratio of 9.5:1, methyltetrahydrophthalic anhydride (purity 99%) is purchased from Sinopharm Chemical Reagent Co., Ltd., and methylnadic anhydride (purity 95%) is purchased from Sinopharm Chemical Reagent Co., Ltd.; wherein, the accelerator is 2-ethyl-4-methylimidazole, both of which are purchased from Sinopharm Chemical Reagent Co., Ltd.

[0090] Preparation of component A: Weigh the raw materials of component A by mass, add the flame retardant prepared in Example 7 to the epoxy resin, stir and mix for 30 min, then add the thermal conductive filler, diluent and toughening agent prepared in Example 3, stir and mix for 40 min, then add the dispersant, defoamer and coupling agent, stir and mix for 20 min, after stirring, evacuate to -0.09 MPa, continue to stir and mix for 50 min, and obtain component A.

[0091] Preparation of component B: Weigh the raw materials of component B according to mass parts, stir and mix the epoxy curing agent and the accelerator for 7 minutes, and after stirring, evacuate to -0.09 Mpa, continue to stir and mix for 25 minutes to obtain component B.

[0092] Preparation of epoxy potting adhesive for chip encapsulation: Component A and component B are stirred and mixed at a rotation speed of 1200 r / min for 4 minutes, wherein the mass ratio of component A to component B is 6:1. After stirring and mixing, the epoxy potting adhesive for chip encapsulation is obtained.

[0093] Comparative Example 1

[0094] Preparation of epoxy potting compound for chip packaging:

[0095] Comparative Example 1 is the control group of Example 8, in which the thermal conductive filler prepared in Example 2 in Example 8 is replaced with hexagonal boron nitride, and the other raw materials and preparation methods remain unchanged, and finally an epoxy potting adhesive for chip packaging is obtained.

[0096] Comparative Example 2

[0097] Preparation of epoxy potting compound for chip packaging:

[0098] Comparative Example 2 is the control group of Example 8, in which the flame retardant prepared in Example 5 in Example 8 is replaced with 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and the other raw materials and preparation methods remain unchanged, and finally an epoxy potting compound for chip packaging is obtained.

[0099] The epoxy potting adhesive for chip encapsulation prepared in Examples 7 to 9 and Comparative Examples 1 to 2 was subjected to a performance test, wherein the curing process was 125° C. / 30 min+165° C. / 90 min. The performance test process was as follows, and the test results are shown in Table 1:

[0100] Hardness: measured in accordance with GB / T 2411-2008 standard;

[0101] Viscosity: measured in accordance with GB / T 2794-2013 standard;

[0102] Tensile strength: measured in accordance with GB / T 6329-1996 standard;

[0103] Breakdown voltage: measured in accordance with GB / T 1408.1-2016 standard;

[0104] Thermal conductivity: measured in accordance with GB / T 10297-2015 standard;

[0105] Limiting oxygen index: measured in accordance with GB / T 2406.1-2008 standard;

[0106] Flame retardant level: measured by the vertical combustion method in accordance with GB / T 2408-2008 standard.

[0107] Table 1

[0108]

[0109] It can be seen from Table 1 that the epoxy potting adhesive for chip packaging prepared in Examples 7 to 9 of the present invention has excellent thermal conductivity, flame retardancy and mechanical properties.

[0110] It should be noted that, in this article, terms such as "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or equipment that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment.

[0111] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing epoxy potting glue for chip packaging, characterized in that: The following steps are involved: S1, adding a flame retardant to the epoxy resin, stirring and mixing, then adding a thermal conductive filler, a diluent and a toughening agent thereto, stirring and mixing, then adding a dispersant, a defoaming agent and a coupling agent thereto, stirring and mixing, after stirring is completed, evacuating, and continuing to stir and mix to obtain component A; S2, stirring and mixing the epoxy curing agent and the accelerator, after stirring, evacuating, and continuing to stir and mix to obtain component B; S3, stirring and mixing component A and component B, and after the stirring and mixing is completed, obtaining an epoxy potting adhesive for chip packaging; The flame retardant is prepared by the following steps: B1: Take chloroform, add vanillin, triethylamine and phosphorus oxychloride to it under nitrogen protection, stir until the solid is completely dissolved, then heat to 40-50°C, stir and react for 24 hours. After the reaction is completed, cool to room temperature, filter, wash the filtrate three times with saturated brine, and then concentrate and crystallize to obtain intermediate 1; B2: Take anhydrous ethanol, add intermediate 1 and ethanolamine to it under nitrogen protection, stir until the solid is completely dissolved, then heat to 50-55°C, stir and react for 4-5 hours. After the reaction is completed, cool to room temperature, and remove anhydrous ethanol by rotary evaporation to obtain intermediate 2; B3: Take 1,4-dioxane, add intermediate II and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide under nitrogen protection, and heat to 70-75°C, stir and react for 4-5 hours. After the reaction is completed, cool to room temperature, filter, take the solid component and wash it three times with 1,4-dioxane to obtain a flame retardant; The mass ratio of the epoxy resin, thermal conductive filler, flame retardant, diluent, toughening agent, dispersant, defoaming agent and coupling agent in S1 is 37-40:15-20:4-7:3-4:12-15:1-2:1-2:1-2; The epoxy curing agent is prepared by mixing methyltetrahydrophthalic anhydride and methylnadic anhydride in a mass ratio of 9.0 to 9.5:1; the accelerator is one of 2-ethylimidazole and 2-ethyl-4-methylimidazole; The thermally conductive filler is prepared by the following steps: A1: Chloroform and sulfonyl chloride are mixed to obtain an activation solution, hexagonal boron nitride is added to the activation solution with stirring, and then ultrasonic stirring is performed for 48 hours at room temperature. After the ultrasonic stirring is completed, vacuum filtration is performed, and the solid component is washed three times with dichloromethane, and then dried at 80-100°C for 12 hours to obtain activated hexagonal boron nitride; A2: Add γ-aminopropyltriethoxysilane to toluene with stirring, heat to 80-100°C, stir at constant temperature for 30 min, then drop deionized water into the mixture, reflux and hydrolyze for 2-4 h. After the reflux and hydrolysis is completed, purify and remove the generated ethanol and unreacted deionized water to obtain a silanol mixed solvent; A3: Stir activated hexagonal boron nitride into toluene, disperse by ultrasonic for 1-2 h, then stir and add silanol mixed solvent, stir and mix for 10-20 min, then add 18% by mass dilute hydrochloric acid to adjust the pH of the system to 6.0-6.5, heat the system to 112-115°C, reflux for 4-5 h, cool to room temperature after the reflux reaction, filter, take the solid component, wash it with anhydrous ethanol and deionized water, and then dry it under vacuum at 80-100°C for 2-4 h to obtain a thermal conductive filler; The volume ratio of chloroform and sulfuryl chloride in A1 is 1:1; The usage ratio of the activation solution and hexagonal boron nitride in A1 is 200 mL:50.0 g; the usage ratio of toluene, γ-aminopropyltriethoxysilane and deionized water in A2 is 100 mL:20 mL:8-10 mL; the usage ratio of toluene, activated hexagonal boron nitride and silanol mixed solvent in A3 is 100 mL:20 g:80-100 mL; The usage ratio of chloroform, vanillin, triethylamine and phosphorus oxychloride described in B1 is 200 mL: 0.2 mol: 0.2 mol: 0.1 mol; the usage ratio of anhydrous ethanol, intermediate 1 and ethanolamine described in B2 is 100 mL: 0.1 mol: 0.1 mol; the usage ratio of 1,4-dioxane, intermediate 2 and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide described in B3 is 100 mL: 0.1 mol: 0.2 mol.

2. The method for preparing an epoxy potting compound for chip packaging according to claim 1, characterized in that: The brand of the epoxy resin is DER-331; the diluent is polyethylene glycol glycidyl dodecyl ether; the toughening agent is WD-401 toughening agent; the dispersant is dispersant BYK-W980; the defoaming agent is one of defoaming agent BYK-054 and defoaming agent BYK-057; and the coupling agent is a mixture of silane coupling agent KH-560 and titanate coupling agent JTW-201 in a mass ratio of 3 to 4:1 to 2.

3. The method for preparing an epoxy potting compound for chip packaging according to claim 1, characterized in that: The mass ratio of the epoxy curing agent to the accelerator in S2 is 10:0.5-1.

0.